A preparation method for a welded and extended super duplex stainless steel seamless pipe coil for a deep-sea umbilical cable, comprising the following steps:
- S1. adding alloying elements to an S32750 super ferritic/austenitic stainless steel base, controlling the composition of liquid steel through triple stripping pretreatment of hot metal and initial refining in an electric arc furnace to produce a qualified molten stainless steel;
- S2. in argon-oxygen refining in an AOD furnace, performing an oxidation reaction to raise the furnace temperature, adding ferrochrome to adjust the composition, adding ferrosilicon during a reduction period to remove CaO+MgO+Al2O3+SiO2 slag from the steel, performing a decarbonization reaction to remove carbon to 0.03% or below so that the composition of liquid steel is stable;
- adding aluminum powder to the slag surface to perform deoxidation so that O element exists in the liquid steel in the form of Al2O3 inclusion;
- preparing high-alkalinity refining slag, and performing calcium treatment for optimization so that Al in the Al2O3 inclusion is replaced by Ca and enters the liquid steel without generating AlN, and the hard non-deforming Al2O3 inclusion is transformed into a plastic calcium aluminate inclusion with a low melting point, wherein the principle of calcium treatment is to generate 12CaO·7 Al2O3 as a liquid inclusion, without the formation of solid CaS inclusion;
- S3. in LF external refining, performing slight argon stirring, adding the high-content MgO+Al2O3 slag and performing deoxidation with aluminum powder to form a high-alkalinity atmosphere, and then further adsorbing inclusions in the liquid steel, and finally casting an ingot by using the liquid steel, wherein the ferrite content in the ingot is controlled to be 45%-56%;
- S4. heating the ingot first, and then performing longitudinal compression on a high-speed forging press followed by transverse compression, so that the ingot is longitudinally compressed with a compression deformation ratio of at least 1;
- after the ingot is forged at least twice on the high-speed forging press, rolling the ingot on a bar hot rolling mill to finally obtain a round billet, wherein the total forging deformation ratio is at least 3.5, the longitudinal drawing deformation ratio is 3.5-5.5, and the total transverse deformation ratio/total longitudinal deformation ratio is 0.30-0.50, and austenitic phase, and the aspect ratio of the austenitic phase is controlled to be 1.0-3.0;
- S5. drilling positioning holes at the center of the round billet, wherein the piercing deformation temperature is 1080° C.-1200° C., the temperature-rise heating time is 150-290 min, and the soaking and holding time is 15-40 min, a high piercing deformation rate weakens the strain distribution effect and increases the dislocation density in the austenitic phase, the piercing rate of super duplex stainless steel can be increased to promote dynamic recrystallization;
- after piercing, the billet is rapidly cooled with water so that the volume fraction of detrimental σ phase in steel is controlled to be at most 0.2%;
- S6. performing cold rolling and solution heat treatment, wherein in a cold-deformation plastic processing process, the deformation of the pony-roughing pass cold-rolled pipe is at most 35-40%, the temperature of solution heat treatment is 1100±10° C., and the holding time is 10-25 min;
- performing a precision large-deformation cold rolling process on a finished product, wherein the deformation of the cold rolled pipe is at most 16-30%, the temperature of solution heat treatment is 1080±10° C., and the holding time is 9-22 min;
- the accumulation of the total deformation of the cold rolled pipe is at least 80%, and the phase ratio is accurately controlled, the ferrite content is controlled to be 49-52%, and the detrimental σ phase in the steel is eliminated;
- and
- S7. performing a self-fusion welding and cosmetic circumferential girth welding process, wherein the outside of the pipe is protected by a high-purity argon-nitrogen mixture (Ar:
- 98% and N2:
- 2%), and the inside of the pipe is protected by pure N2;
- and carrying out polishing and testing, thus obtaining a welded and extended super duplex stainless steel seamless pipe coil.