Abstract
An olivine structured nano-composite LiMxMn1−xPO4/C was synthesized by a sol-gel assisted high energy ball mill method and the synthesis method does not require any inert atmosphere. Electrochemical cycling studies were carried out between 3.0-4.6V using 1M LiPF6 in 1:1 EC/DEC as electrolyte. The charge/discharge cycling studies of the nano-composite exhibit an average discharge capacity of 158 mAh/g at 0.1 C rate over the investigated 50 cycles.
Claims8
A process for the synthesis of high voltage nano composite cathode material LiMxMn1−xPO4/C wherein M is a transition metal cation dopant and x varies from 0 to 0.12 for lithium ion batteries and the said process comprising the steps of:
- i. mixing salts of lithium, manganese, dopant and ammonium dihydrogen orthophosphate in the ratio ranging between 4.1:9.8:0:4.6 to 4.1:8.8:1:4.6;
- ii. dissolving the mixture as obtained in step (i) in water in the ratio ranging between 1:1 at temperature in the range of 27-30° C.;
- iii. adding the solution as obtained in step (ii) in glycine in the ratio ranging between 1:1;
- iv. heating the solution as obtained in step (iii) at temperature in the range of 60 to 75° C. for period in the range of 2 to 4 hours;
- v. drying the heated solution as obtained in step (iv) for period in the range of 10 to 12 hrs at temperature in the range of 100-120° C.;
- vi. grinding and calcining the mixture as obtained in step (v) at temperature in the range of 800-850° C. for period in the range of 4 to 5 hrs in air atmosphere to obtain high voltage nano composite cathode material.
Dependencies are inferred from the claim text.