Forming coated cemented carbide inserts, particularly useful in fine turning of super alloys. The inserts are characterized by a composition of a cemented carbide of WC, about 4.0 wt-% Co to about 7.0 wt-% Co, about 0.25 wt-% Cr to 0.50 wt-% Cr, and a coercivity (Hc) of about 28 kA/m to about 38 kA/m. The coating comprises a single (Ti1-xSix)N-layer, where x is between about 0.1 and about 0.25, with a crystal structure of NaCl type and a total thickness between about 0.5 μm and about 2.0 μm with a strong (200)-texture.
Claims15
A method for making a cutting tool insert having a flank face, comprising a cemented carbide body and a coating, comprising the steps of:
- providing a substrate made by conventional powder metallurgical methods milling, pressing, and sintering with a composition comprising:
- tungsten carbide (WC);
- about 4.0 wt-% to about 7.0 wt-% cobalt (Co);
- about 0.25 wt-% to about 0.50 wt-% chromium (Cr);
- and
- wherein said composition has a coercivity, Hc, of about 28 kA/m to about 38 kA/m;
- and
- depositing a single layer, comprising (Ti1-xSix)N, wherein x is between about 0.1 and about 0.25;
- wherein said layer has a crystal structure of NaCl type and a total thickness of between 0.5 μm and 2.0 μm measured on the middle of said flank face;
- wherein said layer has a texture coefficient TC(200)>about 1.5, the texture coefficient (TC) being defined as:
- TC
-
- (
- hkl
- )
- =
- I
-
- (
- hkl
- )
- I
- 0
-
- (
- hkl
- )
- [
- 1
- n
-
- ∑
- n
- =
- 1
- n
-
-
- I
-
- (
- hkl
- )
- I
- 0
-
- (
- hkl
- )
- ]
- -
- 1
- where:
- I(hkl)=intensity of the (hkl) reflection;
- IO(hkl)=standard intensity according to JCPDS card no 38-1420;
- n=number of reflections used in the calculation;
- (hkl) reflections used are:
- (111), (200), (220),
- using arc evaporation of an alloyed, or Ti+Si composition cathode having a composition comprising:
- about 60 at-% Ti to about 90 at-% Ti, and balance Si;
- with an evaporation current of between about 50 A and about 200 A and a substrate bias of between about −10 V and about −150 V, and a deposition temperature of between about 400° C. and about 700° C., and grown in an Ar+N2 atmosphere comprising about 0 vol-% Ar to about 50 vol-% Ar, at a total pressure of about 0.5 Pa to about 9.0 Pa.
A method for fine wet turning of a superalloy, comprising the steps of:
- providing an insert, said insert comprising:
- a. a cemented carbide body having an edge radius, comprising:
- tungsten carbide (WC);
- about 4.0 wt-% to about 7.0 wt-% cobalt (Co);
- about 0.25 wt-% to about 0.50 wt-% chromium (Cr);
- and
- wherein said cemented carbide body has a coercivity, Hc, of about 28 kA/m to about 38 kA/m;
- and
- a single layer coating comprising (Ti1-xSix)N, wherein x is between about 0.1 and about 0.25;
- wherein said layer has a crystal structure of NaCl type and a total thickness of between 0.5 μm and 2.0 μm measured on the middle of said flank face;
- wherein said layer has a texture coefficient TC(200)>about 1.5, the texture coefficient (TC) being defined as:
- TC
-
- (
- hkl
- )
- =
- I
-
- (
- hkl
- )
- I
- 0
-
- (
- hkl
- )
- [
- 1
- n
-
- ∑
- n
- =
- 1
- n
-
-
- I
-
- (
- hkl
- )
- I
- 0
-
- (
- hkl
- )
- ]
- -
- 1
- where:
- I(hkl)=intensity of the (hkl) reflection;
- IO(hkl)=standard intensity according to JCPDS card no 38-1420;
- n=number of reflections used in the calculation;
- (hkl) reflections used are:
- (111), (200), (220);
- and
- wet cutting said superalloy with said insert at a cutting speed of about 35 m/min to about 130 m/min, a cutting depth of about 0.1 mm to about 0.75 mm, and a feed of about 0.05 mm/rev to about 0.25 mm/rev.
Dependencies are inferred from the claim text.