This invention deals with the concentration process of zinc silicated minerals, particularly willemite and calamine concentration, by single operations, or conventional steps of ore treatment, some of which include the following: Preparation of stockpiles of different mineralogical and contents compositions, crushing, screening, storage, dense separation, washing, homogenization, magnetic separation, grinding, classification, rubbing, conditioning, flotation, thickening, filtering, calcination, storage and waste deposition.
Claims51
Concentration/calcination process of zinc silicated minerals characterized by the following stages, as shown in the block diagrams attached herewith (FIGS. 1, 2, 3 and 4):
- (a) crushing (1) (2):
- Crushing to diminish ore block diameters to around 560 to 38 mm for calamine and around 560 to 15 mm for willemite;
- alternately, ore may previously pass through scalp.
- (b) screening (3) (7) (9):
- In open and closed circuit with crushing to preferentially feed grinding at 100 percent shorter than around 60 mm to around 15 mm in diameter of the ore to be treated.
- (c) storage (4) (5) and dense separation, optional:
- In a revolving drum and sieve.
- (d) washing (6):
- Conventional, under which unders in the trommel are directed to spiral classifiers (10), from which overs, along with the materials caught by the screen (3) (7) (9), are directed to grinding (13) and classifier (14), fines to deslurrying (15) and alternately to homogenization and magnetic separation.
- (e) grinding (13):
- Granulometry material is obtained of nearly 80 to 100 percent under 210 microns that may be directed to rubbing or flotation, or deslurrying, and hydroclone overs feed flotation, and fines are directed to the sump;
- alternately, sieve lump (7) may go for further crushing (8) and a new classification on the sieve (9).
- (f) deslurrying:
- Primary (15), secondary (16), tertiary (17), quaternary (18).
- (g) rubbing (as appropriate):
- Of the pulp using equipment operating at nearly 1500 rpm with 50 to 75 percent pulp weight solids, for 30 to nearly 60 minutes.
- (h) conditioning and additive addition (19) (20):
- Additive is added to ore pulps prior to flotation, firstly pH modifiers, activators, then collectors, frothers, alternately, dispersants and others.
- (i) flotation (21) (22) (23) (24) (25):
- The pulp may be subjected to one or more magnetic separation stages, before, during or after flotation, which may be conducted on conventional or column cells consisting of one or more rougher stages (21), two or more scavengers stages (22) (23) and one or more cleaner stages (24), and cleaner scavenger (25).
- (j) thickening (27):
- Concentrates from different ores were joined to form the final concentrate, which is pumped into one or more thickeners, where one or more flocculants are added at an amount that may range from around 15 to 50 g/t of dry concentrate.
- (k) filtering (28):
- The thickener underflow (27) is filtered and the overflow, after thickening (29), forms an underflow, filtering and an overflow that is settled on the fines concentrate sump. The cake is directed to calcination (31).
- (l) calcination (31):
- The wet cake is fed at a rate that may range from around 500 to 750 t/day wet, on the furnace with inner temperature ranging from around 500 a 1000° C. at the hot zone.
- (m) storage.
Concentrate zinc silicates based product according to earlier claims characterized by the fact that the final calcine concentrate moisture content ranges from nearly 3 to 7 percent and zinc contents from nearly 42 to 47 percent in mass.