AlCuMg alloys with high damage tolerance suitable for use as structural members in aircrafts
AssigneePechiney Rhenalu
InventorsRonan Dif, Timothy Warner, Bernard Bes
Life of this patent
Estimating the term…
Abstract
New alloys for potential use in applications such as in lower wing skins and fuselage skins are disclosed. Specifically, Mn-free 2×24 alloys potentially suitable for thick plate and thin plate and sheet applications are believed to be novel and to provide unexpectedly superior properties.
Claims119
A substantially manganese-free aluminum alloy rolled product consisting essentially of (in percent by weight):
- Cu 3.6-4.5%, Mg 1.0-1.6%, Zr 0.08-0.20%, Sc up to 0.06%, Fe up to 0.08%, Si up to 0.09%, Mn less than 0.05%,remainder aluminum and incident impurities.
An alloy comprising a composition selected from the group consisting of:
- (in weight %)
- 18 Si Fe Cu Mn Mg Ti Zr Sc <0.06 0.06 4.12 0.40 1.37 0.022 <0.06 0.06 3.81 0.008 1.41 0.022 0.109 <0.06 0.07 3.81 0.008 1.36 0.024 0.107 0.028 <0.06 0.05 4.20 0.24 1.23 0.016 0.11 0.032 <0.06 0.06 4.14 0.51 1.24 0.019 0.11 0.032
A substantially manganese-free aluminum alloy rolled product comprising (in percent by weight):
- Cu 3.6-4.5%, Mg 1.0-1.6%, Zr 0.08-0.20%, Sc up to 0.06%, Fe up to 0.08%, Si up to 0.09%, Mn less than 0.05%,remainder aluminum and incident impurities.
A method for obtaining an aluminum alloy rolled product according to claim11, wherein said rolled product comprises a plate, said method comprising:
- Casting a rolling ingot, followed by optional stress relieving, and scalping,
- Homogenizing at a temperature between 450 and 510° C.,
- Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
- Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
- Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
- Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.
A method for obtaining an aluminum alloy rolled product according to claim13, wherein said rolled product comprises a plate, said method comprising:
- Casting a rolling ingot, followed by optional stress relieving, and scalping,
- Homogenizing at a temperature between 450 and 510° C.,
- Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
- Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
- Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
- Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.
An aluminum alloy wherein when employed as plate or sheet, presents a compromise between fracture toughness and mechanical strength in that it is suitable for use in lower wingskin as well as fuselage products,
- wherein when used as a sheet or thin plate fulfilling at least one of the following conditions (i) a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and an apparent fracture toughness Kapp(T-L) of more than 110 MPa{square root}m, measured according to ASTM E 561 in the T-L orientation on a specimen with a width of W=127 mm;
- (ii) an ultimate tensile strength in the longitudinal direction (UTS(L)) of more than 450 MPa, and an elongation at fracture in the longitudinal direction of more than 24%;
- and/or (iii) a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and a Kahn stress Re of at least 180 MPa,,
- and further wherein, when employed as thick plate having at least one the following combinations of properties :
- (i) a UTS(L) of more than 500 MPa, and a Kapp(L-T) of more than 75 MPa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
- (ii) a tensile yield strength in the longitudinal direction (TYS(L)) of more than 450 MPa and a Kapp(L-T) of more than 77 MPa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
- and/or (iii) a tensile yield strength in the longitudinal direction (TYS(L)) of more than 350 MPa and a Kahn stress Re of at least 190 MPa.
Dependencies are inferred from the claim text.