Back to results
US 11,121,282 B2Granted
Method for producing a CdTe thin-film solar cell
AssigneesChina Triumph International Engineering Co., Ltd., Ctf Solar GmbH
InventorsChristian Drost, Sven Frauenstein, Michael Harr, Shou Peng
Life of this patent
Estimating the term…
Abstract
The present invention describes a method for producing CdTe thin-film solar cells, in which special parameters of different processing steps and a special sequence of processing steps result in improved characteristics of the produced CdTe solar cells.
Claims14
A method for producing a CdTe thin film solar cell, the method comprising the steps:
- providing a transparent substrate with a transparent conducting layer as a front contact on it,
- applying a CdS layer on the transparent conducting layer using closed space sublimation technique, wherein the CdS layer is applied with a thickness in the range between 20 nm to 40 nm,
- applying a CdTe layer on the CdS layer using closed space sublimation technique, wherein the CdTe layer is applied with a thickness in the range between 3 μm and 5 μm,
- applying a crystalline layer of CdCl2 with a thickness in the range of 50 nm to 100 nm on a first surface of the CdTe layer,
- performing a first temperature treatment step after applying the CdCl2 layer at a temperature in the range of 380° C. to 430° C. for a time in the range of 15 minutes to 45 minutes under atmospheric conditions,
- performing a first cleaning step after the first temperature treatment step, wherein the layer stack resulting from the previous processing steps is dipped into a solution of diammonium hydrogen citrate with a concentration in the range of 0.1% to 50% for a time in the range of 15 seconds to 5 minutes,
- applying a back contact layer on the first surface after the first cleaning step, wherein the back contact layer is applied with a thickness in the range of 200 nm to 400 nm and comprises molybdenum,
- providing copper ions to a first surface of the back contact layer by dipping a layer stack resulting from the previous process steps into a CuCl2 solution with a concentration in the range of 0.05 mmol/l to 1 mmol/l for a time in the range of 30 seconds to 2 minutes,
- performing a second temperature treatment step after removing the layer stack from the CuCl2 solution at a temperature in the range of 180° C. to 250° C. for a time period with a duration in the range of 10 minutes to 45 minutes under atmospheric conditions,
- performing an artificial aging step after performing the second cleaning step, wherein the artificial aging step includes an illumination of the layer stack resulting from the previous process steps for a time in the range of 1 minute to 48 hours with an illuminance in the range of 5000 lx to 200000 lx at a temperature in the range of 70° C. to 80° C. under atmospheric conditions, and
- performing a second cleaning step after performing the artificial aging step, wherein the layer stack resulting from the previous processing steps is cleaned by dipping the layer stack into a dimethylformamide solution with a concentration in the range of 50% to 100% for a time in the range of 1 minute to 10 minutes and subsequently rinsed with water and isopropanol.
8 more elements
Dependencies are inferred from the claim text.