# US RE37,765 E1 · Process for preparing a nonconductive substrate for electroplating

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US RE37,765 E1
- Document ID: USRE37765E1
- Status: Granted
- Kind: E1
- Application number: 09/255,491
- Filed: 1999-02-22
- Granted: 2002-06-25
- Earliest claimed: 1991-05-01
- Assignees: MacDermid, Incorporated
- Inventors: Catherine M. Randolph; Barry F. Nelsen
- Web page: https://patentgrep.com/patent/USRE37765E1

## Abstract

Described herein is an improved process for electroplating a conductive metal layer to the surface of a nonconductive material comprising pretreating the material with a carbon black dispersion followed by a graphite dispersion before the electroplating step.

## Claims

### Claim 1

A process for electroplating a conductive metal layer to the surface of a nonconductive material, comprising the following steps:
(a) contacting said nonconductive surface with a liquid carbon black dispersion comprising:
(1) carbon black particles having an average particle diameter of less than about 3.0 microns in said dispersion;
(2) an effective dispersing amount of a surfactant which is compatible with said carbon black; and
(3) a first liquid dispersing medium, wherein the amount of carbon black is sufficient to coat substantially all of said nonconducting surfaces and is less than about 4% by weight of said liquid carbon black dispersion;
(b) separating substantially all of said first liquid dispersing medium from said carbon black particles, whereby said particles are deposited on said nonconductive surface in a substantially continuous layer; and
(c) contacting said carbon black-coated nonconductive surface with a liquid conductive graphite dispersion comprising:
(1) conductive graphite particles having an average particle diameter of less than about 1.5 microns in said dispersion;
(2) an effective dispersing amount of a surfactant which is compatible with said conductive graphite; and
(3) a second liquid dispersing medium, wherein the amount of conductive graphite is less than about 4% by weight of said liquid conductive graphite dispersion;
(d) separating substantially all of said second liquid dispersing medium from said conductive graphite particles, whereby said particles are deposited on said carbon black-coated nonconductive surface; and
(e) electroplating a substantially continuous conductive metal layer over the deposited carbon black layer and the deposited conductive graphite layer and said nonconductive surface.

### Claim 2 (depends on 1)

The process of claim 1 wherein said carbon black particles have an average diameter of from about 0.05 to about 3.0 microns.

### Claim 3 (depends on 2)

The process of claim 2 wherein said carbon black particles have an average diameter of from about 0.08 to about 2.0 microns.

### Claim 4 (depends on 1)

The process of claim 1 wherein said graphite particles have an average particle diameter of from about 0.05 to about 0.8 microns.

### Claim 5 (depends on 1)

The process of claim 1 wherein both said first and second liquid dispersing medium are water.

### Claim 6 (depends on 1)

The process of claim 1 wherein said liquid carbon black dispersion contains less than about 10% by weight solids constituents.

### Claim 7 (depends on 1)

The process of claim 1 wherein said liquid graphite dispersion contains less than about 10% by weight solids constituents.

### Claim 8 (depends on 1)

The process of claim 1, wherein said contacting steps (a) and (c) are carried out by immersing the non-conductive material into said liquid carbon black dispersion and liquid conductive graphite dispersion, respectively.

### Claim 9 (depends on 1)

The process of claim 1 wherein said separating steps (b) and (d) are carried out by heating the deposited dispersions.

### Claim 10

The process for electroplating the walls of through holes in a laminated printed wiring board comprised of at least one nonconducting layer laminated to at least two separate conductive metal layers, said process comprising the steps:
(a) contacting said printed wiring board having said through holes in a bath of a liquid carbon black dispersion comprised of:
(1) carbon black particles having an average particle diameter of less than about 3.0 microns in said dispersion;
(2) an effective dispersing amount of a surfactant which is compatible with said carbon black; and
(3) a first liquid dispersing medium wherein the amount of carbon black is sufficient to coat substantially all of said nonconducting surfaces and is less than about 4% by weight of said liquid carbon black dispersion;
(b) separating substantially all of the liquid dispersing medium from said dispersion, thereby depositing said carbon black particles is substantially continuous layer on said nonconducting portions of said hole walls; and
(c) contacting said carbon black-coated printed wiring board with a liquid conductive graphite dispersion comprising:
(1) conductive graphite particles having an average particle diameter of less than about 1.5 microns in said dispersion;
(2) an effective dispersing amount of a surfactant which is compatible with said conductive graphite; and
(3) a second liquid dispersing medium, wherein the amount of conductive graphite is less than about 4% by weight of said liquid conductive graphite dispersion;
(d) separating substantially all of said second liquid dispersing medium from said conductive graphite particles, whereby said particles are deposited on said printed wiring board;
(e) microetching said metal layers of said printed wiring board to remove any deposited carbon black and graphite therefrom; and
(f) electroplating a substantially continuous conductive metal layer over the deposited carbon black layer and the deposited conductive graphite layer on said nonconductive portions of said hole walls, thereby electrically connecting said metal layers of said printed wiring board.

### Claim 11 (depends on 10)

The process of claim 10 wherein said first and second liquid dispersions further comprise a sufficient amount of at least one alkaline hydroxide to raise the pH of said liquid dispersion in the range from about 10 to 14.

### Claim 12 (depends on 11)

The process of claim 11 wherein said alkaline hydroxide is selected from the group consisting of potassium hydroxide, sodium hydroxide, and ammonium hydroxide.

### Claim 13 (depends on 10)

The process of claim 10 wherein said first and second liquid dispersion contain less than about 10% by weight solids constituents.

### Claim 14 (depends on 10)

The process of claim 10 wherein said carbon black particles have an initial pH from about 2 to about 4.

### Claim 15 (depends on 10)

The process of claim 10 wherein said surfactant is a phosphate ester anionic surfactant.

### Claim 16 (depends on 10)

The process of claim 10 wherein said conductive metal is copper.

### Claim 17 (depends on 10)

The process of claim 10 wherein said first and second liquid dispersing medium is water.

### Claim 18 (depends on 10)

The process of claim 10 wherein said process further comprises, before step (a), contacting said printed wiring board with a cleaning solution and a conditioner solution.

### Claim 19 (depends on 18)

The process of claim 18 wherein said process further comprises a water rinse after said microetching step (e).

### Claim 20

A nonconductive surface covered with a deposit of a substantially continuous layer of carbon black having an average particle diameter of less than about 3.0 microns thereon and a layer of conductive graphite having an average particle diameter of less than about 1.5 microns deposited over said carbon black deposit.

### Claim 21 (depends on 20)

The A nonconductive surface of claim 20 covered with a deposit of a substantially continuous layer of carbon black having an average particle diameter of less than about 3.0 microns thereon and a layer of conductive graphite having an average particle diameter of less than about 1.5 microns deposited over said carbon black deposit, wherein said nonconductive surface comprises at least one through hole of a printed wiring board.

### Claim 22

A metal-plated nonconductive surface covered with a deposit of a substantially continuous layer of carbon black having an average particle diameter of less than about 3.0 microns thereon and a layer of conductive graphite having an average particle diameter of less than about 1.5 microns deposited over said carbon black deposit and underlying the plated on metal.

### Claim 23 (depends on 22)

The metal-plated nonconductive surface of claim 22 wherein said nonconductive surface comprises at least one through hole of a printed wiring board.

### Claim 24 (depends on 22)

The metal-plated nonconductive surface of claim 22 wherein said metal is copper.

### Claim 25

A liquid disperson suitable for use in enhancing the electroplating of a nonconducting surface comprised of:
(a) conductive graphite particles having an average particle diameter of less than about 1.5 microns in said dispersion;
(b) an effective dispersing amount of a surfactant which is compatible with said conductive graphite;
(c) optionally, a sufficient amount of at least one alkaline hydroxide to raise the pH of said liquid dispersion in the range from about 9 to 14; and
(d) liquid dispersing medium, wherein the amount of conductive graphite is sufficient to coat substantially all of said nonconducting surface and is less than about 4% by weight of said liquid dispersion and wherein said liquid dispersion contains less than about 10% by weight solids constituents.

### Claim 26 (depends on 25)

The dispersion of claim 25 wherein said alkaline hydroxide is selected from the group consisting of potassium hydroxide, sodium hydroxide, and ammonium hydroxide.

### Claim 27 (depends on 25)

The dispersion of claim 25 wherein said surfactant is a phosphate ester anionic surfactant.

### Claim 28 (depends on 25)

The dispersion of claim 25 wherein said liquid dispersion medium is water.

### Claim 29 (depends on 25)

The dispersion of claim 25 wherein said dispersion further comprises an alkaline hydroxide and said liquid dispersing medium is water, wherein the percentages of each component of said dispersion is as follows:
conductive graphite having an average particle diameter about 0.05-0.8 microns: 0.1-4% by weight
surfactant: 0.01-4% by weight
alkaline hydroxide: 0-1% by weight
water: Balance.

### Claim 30 (depends on 29)

The dispersion of claim 29 wherein said dispersion consists essentially of:
conductive graphite having an average particle diameter of about 0.01-0.4 microns: 0.2-2% by weight
phosphate ester anionic surfactant: 0.05-2% by weight
potassium hydroxide: 0.4-0.8% by weight
water: Balance.