# US 9,353,431 B2 · High-strength aluminum alloy material and process for producing the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 9,353,431 B2
- Document ID: US9353431B2
- Status: Granted
- Kind: B2
- Application number: 14/128,435
- Filed: 2011-08-18
- Published: 2014-05-08
- Granted: 2016-05-31
- Earliest claimed: 2011-06-23
- Assignees: Uacj Corporation
- Applicants: Hidenori Hatta
- Inventors: Hidenori Hatta
- Web page: https://patentgrep.com/patent/US9353431B2

## CPC

- C22F 1/053: of alloys with zinc as the next major constituent
- B21C 23/002: {Extruding materials of special alloys so far as the composition of the alloy requires or permits special extruding methods of sequences}
- C22C 21/00: Alloys based on aluminium
- C22C 21/10: with zinc as the next major constituent
- C22F 1/00: Changing the physical structure of non-ferrous metals or alloys by heat treatment or by hot or cold working (apparatus for mechanical working of metal B21, B23, B24)
- C22F 1/04: of aluminium or alloys based thereon
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- B21C: MANUFACTURE OF METAL SHEETS, WIRE, RODS, TUBES, PROFILES OR LIKE SEMI-MANUFACTURED PRODUCTS OTHERWISE THAN BY ROLLING; AUXILIARY OPERATIONS USED IN CONNECTION WITH METAL-WORKING WITHOUT ESSENTIALLY REMOVING MATERIAL
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

A high-strength aluminum material having a chemical composition which includes Zn: more than 7.2% (mass %, the same applies hereafter) and 8.7% or less, Mg: 1.3% or more and 2.1% or less, Cu: less than 0.50%, Fe: 0.30% or less, Si: 0.30% or less, Mn: less than 0.05%, Cr: 0.20% or less; Zr: less than 0.05%, Ti: 0.001% or more and 0.05% or less, the balance being Al and unavoidable impurities, is provided. It has a proof stress of 350 MPa or more, and a metallographic structure formed of a recrystallized structure. The recrystallized structure is comprised of crystal grains having an average particle diameter of 500 μm or less, and a crystal grain length in a direction parallel to a hot working direction is 0.5 to 4 times as long as a crystal grain length in a direction perpendicular to the hot working direction.

## Claims

### Claim 1

An aluminum alloy material, comprising in mass percent:
Zn: more than 7.2% and 8.7% or less,
Mg: 1.3% or more and 2.1% or less,
Cu: less than 0.50%,
Fe: 0.30% or less,
Si: 0.30% or less,
Mn: less than 0.05%,
Cr: 0.20% or less,
Zr: less than 0.05%,
Ti: 0.001% or more and 0.05% or less,
the balance being Al and unavoidable impurities;
wherein the aluminum alloy material has a proof stress of 350 MPa or more, and a metallographic structure consisting essentially of a recrystallized structure.

### Claim 2 (depends on 1)

The aluminum alloy material according to claim 1, wherein:
the recrystallized structure includes crystal grains having an average particle diameter of 500 μm or less, and
a crystal grain length in a direction parallel to a hot working direction is 0.5 to 4 times as long as a crystal grain length in a direction perpendicular to the hot working direction.

### Claim 3 (depends on 2)

The aluminum alloy material according to claim 2, wherein Zn is more than 7.5% and 8.5% or less.

### Claim 4 (depends on 3)

The aluminum alloy material according to claim 3, wherein Cu is 0.2% or less.

### Claim 5 (depends on 4)

The aluminum alloy material according to claim 4, wherein the crystal grains have an average particle diameter of 50 μm or more.

### Claim 6 (depends on 5)

The aluminum alloy material according to claim 5, wherein the recrystallized structure is a granular recrystallized structure.

### Claim 7 (depends on 1)

The aluminum alloy material according to claim 1, wherein Zn is more than 7.5% and 8.5% or less.

### Claim 8 (depends on 1)

The aluminum alloy material according to claim 1, wherein Cu is 0.2% or less.

### Claim 9 (depends on 1)

The aluminum alloy material according to claim 1, wherein the crystal grains have an average particle diameter of 50 μm or more.

### Claim 10 (depends on 1)

The aluminum alloy material according to claim 1, wherein the recrystallized structure is a granular recrystallized structure.

### Claim 11 (depends on 1)

The aluminum alloy material according to claim 1, wherein Zr is 0.04% or less.

### Claim 12 (depends on 1)

A process for producing the aluminum alloy material according to claim 1, which comprises:
preparing an ingot having a chemical composition which comprises in mass percent Zn: more than 7.2% and 8.7% or less, Mg: 1.3% or more and 2.1% or less, Cu: less than 0.50%, Fe: 0.30% or less, Si: 0.30% or less, Mn: less than 0.05%, Cr: 0.20% or less; Zr: less than 0.05%, Ti: 0.001% or more and 0.05% or less, the balance being Al and unavoidable impurities;
performing a homogenization treatment that heats the ingot at a temperature of higher than 540° C. and 580° C. or lower for 1 hour to 24 hours;
subsequently, forming a wrought material by performing hot working on the ingot in a state where the temperature of the ingot at the beginning of the hot working is 440° C. to 560° C.;
while the wrought material is still at 400° C. or higher, performing a quenching treatment that cools the wrought material to 150° C. or lower;
cooling the temperature of the wrought material to room temperature by said quenching treatment itself or by an additional cooling treatment; and
thereafter, performing an artificial aging treatment that heats the wrought material at a temperature of 100° C. to 170° C. for 5 hours to 30 hours,
wherein the wrought material has a proof stress of 350 MPa or more, and a metallographic structure consisting essentially of a recrystallized structure.

### Claim 13 (depends on 12)

The process according to claim 12, wherein the quenching treatment is performed at a cooling rate of 5° C./sec. to 1000° C./sec.

### Claim 14 (depends on 13)

The process according to claim 13, wherein the cooling rate is 100° C./sec. or more.

### Claim 15 (depends on 14)

The process according to claim 14, wherein the hot working involves extrusion or rolling.

### Claim 16 (depends on 15)

The process according to claim 15, further comprising anodizing the wrought material after the artificial aging treatment.

### Claim 17 (depends on 12)

The process according to claim 12, wherein:
the homogenization treatment is performed at 550° C. for 12 hours,
the hot working comprises subjecting the ingot to extrusion and is initiated while the temperature of the ingot is at 520° C.,
the quenching treatment is initiated while the temperature of the wrought material is at 505° C. and the cooling rate of the quenching treatment is 600° C./sec, and
the artificial aging treatment involves heating the wrought material at 150° C. for 12 hours.

### Claim 18 (depends on 17)

The process according to claim 17, further comprising anodizing the wrought material after the artificial aging treatment.

### Claim 19 (depends on 12)

The process according to claim 12, further comprising anodizing the wrought material after the artificial aging treatment.

### Claim 20 (depends on 1, 5)

A process for producing the aluminum alloy material of claim 1, comprising:
homogenizing an ingot having the elemental composition recited in claim 5 at a temperature of higher than 540° C. and 580° C. or lower for at least 1 hour;
hot working the homogenized ingot, the hot working being initiated while the temperature of the homogenized ingot it 440° C. to 560° C.;
quenching hot worked material to 150° C. or lower, the quenching being initiated while the hot worked material is at a temperature of 400° C. or higher,
cooling the hot worked material to room temperature; and
subjecting the cooled material to an artificial aging treatment at a temperature of 100° C. to 170° C. for 5 hours to 30 hours,
wherein the aluminum alloy material has a proof stress of 350 MPa or more, and a metallographic structure consisting essentially of a recrystallized structure.