# US 9,353,426 B2 · Silver-white copper alloy and method of producing silver-white copper alloy

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 9,353,426 B2
- Document ID: US9353426B2
- Status: Granted
- Kind: B2
- Application number: 14/069,086
- Filed: 2013-10-31
- Published: 2014-05-08
- Granted: 2016-05-31
- Earliest claimed: 2011-06-29
- Assignees: Mitsubishi Materials Corporation; Mitsubishi Shindoh Co., Ltd.
- Applicants: Mitsubishi Shindoh Co., Ltd.; Mitsubishi Materials Corporation
- Inventors: Shinji Tanaka; Keiichiro Oishi; Hiroharu Ogawa
- Web page: https://patentgrep.com/patent/US9353426B2

## CPC

- C22C 9/04: with zinc as the next major constituent
- C22F 1/08: of copper or alloys based thereon
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

Provided are a silver-white copper alloy which has superior mechanical properties such as hot workability, cold workability, or press property, color fastness, bactericidal and antibacterial properties, and Ni allergy resistance; and a method of producing such a silver-white copper alloy. The silver-white copper alloy includes 51.0 mass % to 58.0 mass % of Cu; 9.0 mass % to 12.5 mass % of Ni; 0.0003 mass % to 0.010 mass % of C; 0.0005 mass % to 0.030 mass % of Pb; and the balance of Zn and inevitable impurities, in which a relationship of 65.5≦[Cu]+1.2×[Ni]≦70.0 is satisfied between a content of Cu [Cu] (mass %) and a content of Ni [Ni] (mass %). In a metal structure thereof, an area ratio of β phases dispersed in an α-phase matrix is 0% to 0.9%.

## Claims

### Claim 1

A method of producing a silver-white copper alloy, comprising the steps of:
(a) providing a silver-white copper alloy, comprising:
51.0 mass % to 57.0 mass % of Cu,
9.0 mass % to 12.5 mass % of Ni,
0.0003 mass % to 0.010 mass % of C,
0.0005 mass % to 0.030 mass % of Pb, and
with a balance of Zn and inevitable impurities,
and satisfying a relationship of 65.5≦[Cu]+1.2×[Ni]≦69.0 between an amount of Cu [Cu] (mass %) and an amount of Ni [Ni] (mass %),
and satisfying a relationship of 0.58≦[Zn]/[Cu]<0.7 between an amount of Cu [Cu] (mass %) and an amount of Zn [Zn] (mass %);
(b) hot-rolling the silver-white copper alloy; and
(c) cooling the hot-rolled silver-white copper alloy without quenching from a temperature immediately after the hot-rolling to a room temperature, wherein a cooling rate of the hot-rolled silver-white copper alloy in a temperature range of 400° C. to 500° C. is higher than or equal to 1° C./sec to provide a metal structure of the silver-white copper alloy having an area ratio of β phases dispersed in an α-phase matrix is 0% to 0.9%,
wherein the silver-white copper alloy has superior bactericidal and color fastness properties.

### Claim 2 (depends on 1)

The method of producing a silver-white copper alloy according to claim 1,
wherein the silver-white copper alloy further comprises one or more selected from a group consisting of 0.01 mass % to 0.3 mass % of Al, 0.005 mass % to 0.09 mass % of P, 0.01 mass % to 0.09 mass % of Sb, 0.01 mass % to 0.09 mass % of As, and 0.001 mass % to 0.03 mass % of Mg.

### Claim 3

A method of producing a silver-white copper alloy, comprising:
heating a rolled silver-white copper alloy to a predetermined temperature by using a continuous annealing line, thereby defining a heat treatment process, maintaining the rolled silver-white copper alloy at a predetermined temperature for a predetermined time, and cooling the rolled silver-white copper alloy to a predetermined temperature,
wherein, when a maximum achieved temperature of the rolled silver-white copper alloy in the heat treatment process is represented by Tmax (° C.) and a retention time of the heat treatment process in a temperature range from a temperature, which is 50° C. lower than the maximum achieved temperature of the rolled silver-white copper alloy, to the maximum achieved temperature is represented by th (min), expressions of 520≦Tmax≦800, 0.1≦th≦50, and 470≦Tmax−90×th−1/2≦620 are satisfied and a cooling rate during the cooling of the rolled silver-white copper alloy in a temperature range of 400° C. to 500° C. is higher than or equal to 1° C./sec,
wherein the silver-white copper alloy comprises:
51.0 mass % to 57.0 mass % of Cu,
9.0 mass % to 12.5 mass % of Ni,
0.0003 mass % to 0.010 mass % of C,
0.0005 mass % to 0.030 mass % of Pb, and
with a balance of Zn and inevitable impurities,
satisfying a relationship of 65.55≦[Cu]+1.2×[Ni]≦69.0 between an amount of Cu [Cu] (mass %) and an amount of Ni [Ni] (mass %),
wherein a relationship of 0.58≦[Zn]/[Cu]<0.7 is satisfied between an amount of Cu [Cu] (mass %) and an amount of Zn [Zn] (mass %),
wherein subsequent to cooling the silver-white copper alloy has a metal structure having an area ratio of (3 phases dispersed in an α-phase matrix is from 0% to 0.9%, and
wherein the silver-white copper alloy has superior bactericidal and color fastness properties.

### Claim 4 (depends on 3)

The method of producing a silver-white copper alloy according to claim 3,
wherein the silver-white copper alloy further comprises one or more selected from a group consisting of 0.01 mass % to 0.3 mass % of Al, 0.005 mass % to 0.09 mass % of P, 0.01 mass % to 0.09 mass % of Sb, 0.01 mass % to 0.09 mass % of As, and 0.001 mass % to 0.03 mass % of Mg.

### Claim 5

A method of producing a silver-white copper alloy, comprising:
cooling a hot-rolled silver-white copper alloy without quenching from a temperature immediately after the hot-rolling to a room temperature, wherein a cooling rate of the hot-rolled silver-white copper alloy in a temperature range of 400° C. to 500° C. is higher than or equal to 1° C./sec,
wherein the silver-white copper alloy comprises:
51.0 mass % to 57.0 mass % of Cu,
9.0 mass % to 12.5 mass % of Ni,
0.05 mass % to 0.9 mass % of Mn,
0.0003 mass % to 0.010 mass % of C,
0.0005 mass % to 0.030 mass % of Pb, and
a balance of Zn and inevitable impurities,
satisfying a relationship of 65.5≦[Cu]+1.2×[Ni]+0.4×[Mn]≦69.0 between an amount of Cu [Cu] (mass %), an amount of Ni [Ni] (mass %), and an amount of Mn [Mn] (mass %),
wherein a relationship of 0.58≦[Zn]/[Cu]<0.7 is satisfied between an amount of Cu [Cu] (mass %) and an amount of Zn [Zn] (mass %),
wherein in a metal structure thereof, an area ratio of β phases dispersed in an α-phase matrix is 0% to 0.9%, and
wherein the silver-white copper alloy has superior bactericidal and color fastness properties.

### Claim 6 (depends on 5)

The method of producing a silver-white copper alloy according to claim 5,
wherein the silver-white copper alloy further comprises one or more selected from a group consisting of 0.01 mass % to 0.3 mass % of Al, 0.005 mass % to 0.09 mass % of P, 0.01 mass % to 0.09 mass % of Sb, 0.01 mass % to 0.09 mass % of As, and 0.001 mass % to 0.03 mass % of Mg.

### Claim 7

A method of producing a silver-white copper alloy, comprising:
heating a rolled silver-white copper alloy to a predetermined temperature by using a continuous annealing line;
maintaining the rolled silver-white copper alloy at a predetermined temperature for a predetermined time; and
cooling the rolled silver-white copper alloy to a predetermined temperature,
wherein, when a maximum achieved temperature of the rolled silver-white copper alloy in the heat treatment process is represented by Tmax (° C.) and a retention time of the heat treatment process in a temperature range from a temperature, which is 50° C. lower than the maximum achieved temperature of the rolled silver-white copper alloy, to the maximum achieved temperature is represented by th (min), expressions of 520≦Tmax≦800, 0.1≦th≦50, and 470≦Tmax−90×th−1/2≦620 are satisfied and a cooling rate during the cooling of the rolled silver-white copper alloy in a temperature range of 400° C. to 500° C. is higher than or equal to 1° C./sec,
wherein the silver-white copper alloy comprises:
51.0 mass % to 57.0 mass % of Cu,
9.0 mass % to 12.5 mass % of Ni,
0.05 mass % to 0.9 mass % of Mn,
0.0003 mass % to 0.010 mass % of C2
0.0005 mass % to 0.030 mass % of Pb, and
the balance of Zn and inevitable impurities,
satisfying a relationship of 65.5≦[Cu]+1.2×[Ni]+0.4×[Mn]≦9.0 between an amount of Cu [Cu] (mass %), an amount of Ni [Ni] (mass %), and an amount of Mn [Mn] (mass %),
wherein a relationship of 0.58≦[Zn]/[Cu]<0.7 is satisfied between an amount of Cu [Cu] (mass %) and an amount of Zn [Zn] (mass %),
wherein in a metal structure thereof, an area ratio of β phases dispersed in an α-phase matrix is 0% to 0.9%, and
wherein the silver-white copper alloy has superior bactericidal and color fastness properties.

### Claim 8 (depends on 7)

The method of producing a silver-white copper alloy according to claim 7,
wherein the silver-white copper alloy further comprises one or more selected from a group consisting of 0.01 mass % to 0.3 mass % of Al, 0.005 mass % to 0.09 mass % of P, 0.01 mass % to 0.09 mass % of Sb, 0.01 mass % to 0.09 mass % of As, and 0.001 mass % to 0.03 mass % of Mg.

### Claim 9

A method of producing a silver-white copper alloy, comprising
cooling a hot-rolled silver-white copper alloy without quenching from a temperature immediately after the hot-rolling to a room temperature, wherein a cooling rate of a hot-rolled silver-white copper alloy in a temperature range of 400° C. to 500° C. is higher than or equal to 1° C./sec,
wherein the silver-white copper alloy comprises:
51.5 mass % to 57.0 mass % of Cu,
10.0 mass % to 12.0 mass % of Ni,
0.05 mass % to 0.9 mass % of Mn,
0.0005 mass % to 0.008 mass % of C,
0.001 mass % to 0.009 mass % of Pb, and
with a balance of Zn and inevitable impurities,
satisfying a relationship of 66.0≦[Cu]+1.2×[Ni]+0.4×[Mn]≦68.0 between an amount of Cu [Cu] (mass %), an amount of Ni [Ni] (mass %), and an amount of Mn [Mn] (mass %),
wherein a relationship of 0.58≦[Zn]/[Cu]<0.7 is satisfied between an amount of Cu [Cu] (mass %) and an amount of Zn [Zn] (mass %),
wherein in a metal structure thereof, an area ratio of β phases dispersed in an α-phase matrix is 0% to 0.4%, and
wherein the silver-white copper alloy has superior bactericidal and color fastness properties.

### Claim 10 (depends on 9)

The method of producing a silver-white copper alloy according to claim 9,
wherein the silver-white copper alloy further comprises one or more selected from a group consisting of 0.01 mass % to 0.3 mass % of Al, 0.005 mass % to 0.09 mass % of P, 0.01 mass % to 0.09 mass % of Sb, 0.01 mass % to 0.09 mass % of As, and 0.001 mass % to 0.03 mass % of Mg.

### Claim 11

A method of producing a silver-white copper alloy, comprising:
heating a rolled silver-white copper alloy to a predetermined temperature by using a continuous annealing line;
maintaining the rolled silver-white copper alloy at a predetermined temperature for a predetermined time; and
cooling the rolled silver-white copper alloy to a predetermined temperature,
wherein, when a maximum achieved temperature of the rolled silver-white copper alloy in the heat treatment process is represented by Tmax (° C.) and a retention time of the heat treatment process in a temperature range from a temperature, which is 50° C. lower than the maximum achieved temperature of the rolled silver-white copper alloy, to the maximum achieved temperature is represented by th (min), expressions of 520≦Tmax≦800, 0.1≦th≦50, and 470≦Tmax−90×th−1/2≦620 are satisfied and a cooling rate during the cooling of the rolled silver-white copper alloy in a temperature range of 400° C. to 500° C. is higher than or equal to 1° C./sec,
wherein the silver-white copper alloy comprises:
51.5 mass % to 57.0 mass % of Cu,
10.0 mass % to 12.0 mass % of Ni,
0.05 mass % to 0.9 mass % of Mn,
0.0005 mass % to 0.008 mass % of C,
0.001 mass % to 0.009 mass % of Pb, and
with a balance of Zn and inevitable impurities,
satisfying a relationship of 66.0≦[Cu]+1.2×[Ni]+0.4×[Mn]≦68.0 between an amount of Cu [Cu] (mass %), an amount of Ni [Ni] (mass %), and an amount of Mn [Mn] (mass %),
wherein a relationship of 0.58≦[Zn]/[Cu]<0.7 is satisfied between an amount of Cu [Cu] (mass %) and an amount of Zn [Zn] (mass %),
wherein in a metal structure thereof, an area ratio of β phases dispersed in an α-phase matrix is 0% to 0.4%, and
wherein the silver-white copper alloy has superior bactericidal and color fastness properties.

### Claim 12 (depends on 11)

The method of producing a silver-white copper alloy according to claim 11,
wherein the silver-white copper alloy further comprises one or more selected from a group consisting of 0.01 mass % to 0.3 mass % of Al, 0.005 mass % to 0.09 mass % of P, 0.01 mass % to 0.09 mass % of Sb, 0.01 mass % to 0.09 mass % of As, and 0.001 mass % to 0.03 mass % of Mg.

### Claim 13

A method of producing a silver-white copper alloy, comprising:
heating a rolled silver-white copper alloy to a predetermined temperature by using a continuous annealing line, thereby defining a heat treatment process, maintaining the rolled silver-white copper alloy at a predetermined temperature for a predetermined time, and cooling the rolled silver-white copper alloy to a predetermined temperature,
wherein, when a maximum achieved temperature of the rolled silver-white copper alloy in the heat treatment process is represented by Tmax (° C.) and a retention time of the heat treatment process in a temperature range from a temperature, which is 50° C. lower than the maximum achieved temperature of the rolled silver-white copper alloy, to the maximum achieved temperature is represented by th (min), expressions of 680≦Tmax≦730, 0.25≦th≦0.5, and 470≦Tmax−90×th−1/2≦620 are satisfied and a cooling rate during the cooling of the rolled silver-white copper alloy in a temperature range of 400° C. to 500° C. is higher than or equal to 1° C./sec, without quenching from a temperature immediately after the heat treatment process to a room temperature,
wherein the silver-white copper alloy comprises:
51.0 mass % to 57.0 mass % of Cu,
9.0 mass % to 12.5 mass % of Ni,
0.0003 mass % to 0.010 mass % of C,
0.0005 mass % to 0.030 mass % of Pb, and
with a balance of Zn and inevitable impurities,
satisfying a relationship of 65.5≦[Cu]+1.2×[Ni]≦69.0 between an amount of Cu [Cu] (mass %) and an amount of Ni [Ni] (mass %),
wherein a relationship of 0.58≦[Zn]/[Cu]<0.7 is satisfied between an amount of Cu [Cu] (mass %) and an amount of Zn [Zn] (mass %);
wherein subsequent to cooling the silver-white copper alloy has a metal structure having an area ratio of β phases dispersed in an α-phase matrix is from 0% to 0.9%, and
wherein the silver-white copper alloy has superior bactericidal and color fastness properties.