# US 9,352,360 B2 · Ceramic wear tile and method of using same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 9,352,360 B2
- Document ID: US9352360B2
- Status: Granted
- Kind: B2
- Application number: 14/300,485
- Filed: 2014-06-10
- Published: 2014-09-25
- Granted: 2016-05-31
- Earliest claimed: 2013-06-19
- Assignees: Cerco LLC
- Applicants: CerCo LLC
- Inventors: Gary C. Troyer
- Web page: https://patentgrep.com/patent/US9352360B2

## CPC

- B07C 5/3425: {of granular material, e.g. ore particles, grain (investigation moving fluids or granular solids using optical means G01N21/85)}
- B07C 5/342: according to optical properties, e.g. colour {(according to radiation transmittivity B07C5/3416)}
- C04B 35/10: based on aluminium oxide
- F27B 9/20: the charge moving in a substantially straight path
- C04B 35/111: Fine ceramics
- C04B 2235/3217: Aluminum oxide or oxide forming salts thereof, e.g. bauxite, alpha-alumina
- C04B 2235/3232: Titanium oxides or titanates, e.g. rutile or anatase
- C04B 2235/3241: Chromium oxides, chromates, or oxide-forming salts thereof
- C04B 2235/3243: Chromates or chromites, e.g. aluminum chromate, lanthanum strontium chromite
- C04B 2235/3262: Manganese oxides, manganates, rhenium oxides or oxide-forming salts thereof, e.g. MnO
- C04B 2235/3263: Mn3O4
- C04B 2235/3265: Mn2O3
- C04B 2235/3267: MnO2
- C04B 2235/3268: Manganates, manganites, rhenates or rhenites, e.g. lithium manganite, barium manganate, rhenium oxide
- C04B 2235/3272: Iron oxides or oxide forming salts thereof, e.g. hematite, magnetite
- C04B 2235/3274: Ferrites
- C04B 2235/3463: Alumino-silicates other than clay, e.g. mullite
- C04B 2235/349: Clays, e.g. bentonites, smectites such as montmorillonite, vermiculites or kaolines, e.g. illite, talc or sepiolite
- C04B 2235/445: Fluoride containing anions, e.g. fluosilicate
- Y10T 29/49826: Assembling or joining
- Y10T 156/10: Methods of surface bonding and/or assembly therefor
- B07C: POSTAL SORTING; SORTING INDIVIDUAL ARTICLES, OR BULK MATERIAL FIT TO BE SORTED PIECE-MEAL, e.g. BY PICKING (specially adapted for a specific purpose covered by another class, see the relevant place, e.g. A43D33/06, B23Q7/12)
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- F27B: FURNACES, KILNS, OVENS OR RETORTS IN GENERAL; OPEN SINTERING OR LIKE APPARATUS
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

The present subject matter provides colored wear tiles for use in optical sorting apparatuses and related methods that separate an associated material into a desired product and an undesired product. The colored wear tiles have a color and/or lightness value that permeates the entire body of the wear tile and sufficiently differs from the color and/or lightness of the associated material in order to allow the colored wear tile, or portions or pieces thereof, that may mix with the associated material, to be separated from the desired product by the sorting apparatus.

## Claims

### Claim 1

A colored wear tile for inhibiting wear to a surface, the wear being associated to contact with a moving material, wherein:
the colored wear tile comprises prior to firing, non-volatile components comprising at least 85 wt. % Al2O3;
the colored wear tile has a color that permeates substantially an entire mass of the colored wear tile;
the colored wear tile has a Vickers hardness from about 900HV5 to about 1350HV5;
the colored wear tile has a thickness of less than about 0.60 inches;
the colored wear tile has a lightness of about 90 or less measured with a CIE D65 illuminant at 10 degrees; and
the colored wear tile is brown and is produced by firing a composition at or above about 2500° F. from about 45 minutes to about 90 minutes, the composition comprising prior to firing:
a. Al2O3 from about 75 wt. % to about 98 wt. %,
b. MnO2 from about 0.25 wt. % to about 3.5 wt. %,
c. TiO2 from about 0.1 wt. % to about 2.5 wt. %,
d. Fe3O4 from about 0.1 wt. % to about 2.5 wt. %,
e. clay from about 0 wt. % to about 10 wt. %,
f. Al2SiO5 from about 0.01 wt. % to about 8.0 wt. %,
g. talc from about 0 wt. % to about 2.5 wt. %,
h. dispersant from about 0 wt. % to about 2.0 wt. %,
i. defoamer from about 0 wt. % to about 1.0 wt. %,
j. binder from about 0.1 wt. % to about 10 wt. %, and
k. calcium stearate from about 0 wt. % to about 4.5 wt. %.

### Claim 2 (depends on 1)

The colored wear tile according to claim 1, wherein the composition comprises prior to firing:
a. Al2O3 from about 75 wt. % to about 98 wt. %,
b. MnO2 from about 0.5 wt. % to about 2.0 wt. %,
c. TiO2 from about 0.1 wt. % to about 1.5 wt. %,
d. Fe3O4 from about 0.1 wt. % to about 1.5 wt. %,
e. clay from about 1.0 wt. % to about 3.5 wt. %,
f. Al2SiO5 from about 0.5 wt. % to about 6.0 wt. %,
g. talc from about 0.2 wt. % to about 1.5 wt. %,
h. dispersant from about 0.2 wt. % to about 0.6 wt. %,
i. defoamer from about 0.05 wt. % to about 0.2 wt. %,
j. binder from about 0.5 wt. % to about 8.0 wt. %, and
k. calcium stearate from about 0.3 wt. % to about 3.5 wt. %.

### Claim 3

A colored wear tile for inhibiting wear to a surface, the wear being associated to contact with a moving material, wherein:
the colored wear tile comprises prior to firing, non-volatile components comprising at least 85 wt. % Al2O3;
the colored wear tile has a color that permeates substantially an entire mass of the colored wear tile;
the colored wear tile has a Vickers hardness from about 900HV5 to about 1350HV5;
the colored wear tile has a thickness of less than about 0.60 inches;
the colored wear tile has a lightness of about 90 or less measured with a CIE D65 illuminant at 10 degrees; and
the colored wear tile is pink and is produced by firing a composition at or above about 2500 ° F. from about 45 minutes to about 90 minutes, the composition comprising prior to firing:
a. Al2O3 from about 75 wt. % to about 98 wt. %,
b. CaF2 from about 0.1 wt. % to about 4.0 wt. %,
c. Cr2O3 from about 0.05 wt. % to about 3.0 wt. %,
d. clay from about 0 wt. % to about 4.5 wt. %,
e. talc from about 0 wt. % to about 4.0 wt. %,
f. tannic acid from about 0 wt. % to about 3.5 wt. %,
g. dispersant from about 0 wt. % to about 3.0 wt. %,
h. defoamer from about 0 wt. % to about 2.0 wt. %,
i. binder from about 0 wt. % to about 10.0 wt. %, and
j. calcium stearate from about 0 wt. % to about 4.5 wt. %.

### Claim 4 (depends on 3)

The colored wear tile according to claim 3, wherein the composition comprises prior to firing:
a. Al2O3 from about 75 wt. % to about 98 wt. %,
b. CaF2 from about 0.5 wt. % to about 3.0 wt. %,
c. Cr2O3 from about 0.1 wt. % to about 2.0 wt. %,
d. clay from about 1.0 wt. % to about 3.5 wt. %,
e. talc from about 0.2 wt. % to about 3.0 wt. %,
f. tannic acid from about 0.05 wt. % to about 2.0 wt. %,
g. dispersant from about 0.2 wt. % to about 1.0 wt. %,
h. defoamer from about 0.02 wt. % to about 0.2 wt. %,
i. binder from about 0.7 wt. % to about 7.5 wt. %, and
j. calcium stearate from about 0.1 wt. % to about 3.5 wt. %.

### Claim 5

A colored wear tile for inhibiting wear to a surface, the wear being associated to contact with a moving material, wherein:
the colored wear tile comprises prior to firing, non-volatile components comprising at least 85 wt. % Al2O3;
the colored wear tile has a color that permeates substantially an entire mass of the colored wear tile;
the colored wear tile has a Vickers hardness from about 900HV5 to about 1350HV5;
the colored wear tile has a thickness of less than about 0.60 inches;
the colored wear tile has a lightness of about 90 or less measured with a CIE D65 illuminant at 10 degrees; and
the colored wear tile is pink and is produced by firing a composition at or above about 2500 ° F. from about 45 minutes to about 90 minutes, the composition comprising prior to firing:
a. Al2O3 from about 75 wt. % to about 98 wt. %,
b. Al2SiO5 from about 0.01 wt. % to about 8.0 wt. %,
c. Cr2O3 from about 0.05 wt. % to about 3.0 wt. %,
d. clay from about 0 wt. % to about 10.0 wt. %,
e. talc from about 0 wt. % to about 4.0 wt. %,
f. Stonelite (CaMg(CO3)2-Fe2O3) or dolomite (CaMg(CO3)2) from about 0 wt. % to about 3.5 wt. %,
g. dispersant from about 0 wt. % to about 3.0 wt. %,
h. defoamer from about 0 wt. % to about 2.0 wt. %,
i. binder from about 0 wt. % to about 10.0 wt. %, and
j. calcium stearate from about 0 wt. % to about 4.5 wt. %.

### Claim 6

A colored wear tile for inhibiting wear to a surface, the wear being associated to contact with a moving material, wherein:
the colored wear tile comprises prior to firing, non-volatile components comprising at least 85 wt. % Al2O3;
the colored wear tile has a color that permeates substantially an entire mass of the colored wear tile;
the colored wear tile has a Vickers hardness from about 900HV5 to about 1350HV5;
the colored wear tile has a thickness of less than about 0.60 inches;
the colored wear tile has a lightness of about 90 or less measured with a CIE D65 illuminant at 10 degrees; and
the colored wear tile is blue and is produced by firing a composition at or above about 2500 ° F. from about 45 minutes to about 90 minutes, the composition comprising prior to firing:
a. Al2O3 from about 75 wt. % to about 98 wt. %,
b. Al2SiO5 from about 0.5 wt. % to about 8.0 wt. %,
c. clay from about 0 wt. % to about 10.0 wt. %,
d. talc from about 0 wt. % to about 4.0 wt. %,
e. Stonelite (CaMg(CO3)2-Fe2O3) or dolomite (CaMg(CO3)2) from about 0 wt. % to about 3.5 wt. %,
f. CoO from about 0 wt. % to about 3.0 wt. %,
g. dispersant from about 0 wt. % to about 3.0 wt. %,
h. defoamer from about 0 wt. % to about 2.0 wt. %,
i. binder from about 0 wt. % to about 5.0 wt. %, and
j. calcium stearate from about 0 wt. % to about 3.5 wt. %.

### Claim 7

A colored wear tile for inhibiting wear to a surface, the wear being associated to contact with a moving material, wherein:
the colored wear tile comprises prior to firing, non-volatile components comprising at least 85 wt. % Al2O3;
the colored wear tile has a color that permeates substantially an entire mass of the colored wear tile;
the colored wear tile has a Vickers hardness from about 900HV5 to about 1350HV5;
the colored wear tile has a thickness of less than about 0.60 inches;
the colored wear tile has a lightness of about 90 or less measured with a CIE D65 illuminant at 10 degrees; and
the colored wear tile is black and is produced by firing a composition at or above about 2500 ° F. from about 45 minutes to about 90 minutes, the composition comprising prior to firing:
a. Al2O3 from about 75 wt. % to about 98 wt. %,
b. TiO2 from about 0.5 wt. % to about 5.0 wt. %,
c. CoO from about 0 wt. % to about 3.0 wt. %,
d. Fe3O4 from about 0 wt. % to about 3.0 wt. %,
e. NiO2 from about 0 wt. % to about 3.0 wt. %,
f. Kaolin clay (Al2Si2O5(OH)4) from about 1.0 wt. % to about 8.0 wt. %,
g. dispersant from about 0 wt. % to about 3.0 wt. %,
h. defoamer from about 0 wt. % to about 2.0 wt. %,
i. binder from about 0 wt. % to about 5.0 wt. %, and
j. calcium stearate from about 0 wt. % to about 3.5 wt. %.