# US 8,999,869 B2 · Glass-ceramic joining material and use thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 8,999,869 B2
- Document ID: US8999869B2
- Status: Granted
- Kind: B2
- Application number: 13/867,223
- Filed: 2013-04-22
- Published: 2013-11-07
- Granted: 2015-04-07
- Earliest claimed: 2012-05-04
- Assignees: Schott AG
- Applicants: Schott AG
- Inventors: Dieter Goedeke
- Web page: https://patentgrep.com/patent/US8999869B2

## CPC

- G03C 8/24: Photosensitive materials characterised by the image-receiving section
- C03C 3/064: containing boron
- C03C 8/24: Fusion seal compositions being frit compositions having non-frit additions, i.e. for use as seals between dissimilar materials, e.g. glass and metal; Glass solders
- C03C 10/0036: {containing SiO2, Al2O3 and a divalent metal oxide as main constituents}
- C25B 9/00: Cells or assemblies of cells; Constructional parts of cells; Assemblies of constructional parts, e.g. electrode-diaphragm assemblies; Process-related cell features
- H01M 8/0282: Inorganic material
- Y02E 60/50: Fuel cells
- Y10T 403/477: Fusion bond, e.g., weld, etc.
- G03C: PHOTOSENSITIVE MATERIALS FOR PHOTOGRAPHIC PURPOSES (for photomechanical purposes G03F); PHOTOGRAPHIC PROCESSES, e.g. CINE, X-RAY, COLOUR, STEREO-PHOTOGRAPHIC PROCESSES; AUXILIARY PROCESSES IN PHOTOGRAPHY (photographic processes characterised by the use or manipulation of apparatus classifiable per se in subclass G03B, see G03B; photomechanical production of textured or patterned surfaces G03F; electrophotography, magnetography G03G)
- C03C: CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
- C25B: ELECTROLYTIC OR ELECTROPHORETIC PROCESSES FOR THE PRODUCTION OF COMPOUNDS OR NON-METALS; APPARATUS THEREFOR (anodic or cathodic protection C23F13/00; single-crystal growth C30B)
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

The glass-ceramic joining material, which is suitable for bonding or joining at low processing temperatures, especially less than 800° C., is composed of a BaO—SiO2—CaO—B2O3—Al2O3 system and has a coefficient of thermal expansion α(20-300)≧9.5·10−6 K−1.

## Claims

### Claim 1

An article comprising a bond between at least two metal components;
wherein said bond comprises a glass-ceramic joining material and said metal components are joined by said joining material;
wherein said glass-ceramic joining material has a coefficient of thermal expansion α(20-300)≧9.5·10−6 K−1; and
wherein said glass-ceramic joining material, apart from at most impurities, is free of ZnO and free of PbO, and comprises, in mol % based on oxide content:
SiO2
3-<10
B2O3
16-34
Al2O3
7-15
CaO
8-40
BaO
25-38
MgO
0-10
ZrO2
0-5
Y2O3
0-10.

### Claim 2

An article comprising a bond between at least two metal components;
wherein said bond comprises a glass-ceramic joining material and said metal components are joined by said joining material; and
wherein said metal components are composed of ferritic stainless steel;
wherein said glass-ceramic joining material has a coefficient of thermal expansion α(20-300)≧9.5·10−6 K−1; and
wherein said glass-ceramic joining material, apart from at most impurities, is free of ZnO and free of PbO, and comprises, in mol% based on oxide content:
SiO2
3-<10
B2O3
16-34
Al2O3
7-15
CaO
8-40
BaO
25-38
MgO
0-10
ZrO2
0-5
Y2O3
0-10.

### Claim 3

An article comprising a bond between at least two ceramic components;
wherein said bond comprises a glass-ceramic joining material and said ceramic components are joined by said joining material;
wherein said glass-ceramic joining material has a coefficient of thermal expansion α(20-300)≧9.5·10−6 K−1; and
wherein said glass-ceramic joining material, apart from at most impurities, is free of ZnO and free of PbO, and comprises, in mol% based on oxide content:
SiO2
3-<10
B2O3
16-34
Al2O3
7-15
CaO
8-40
BaO
25-38
MgO
0-10
ZrO2
0-5
Y2O3
0-10.

### Claim 4

An article comprising a bond between at least two ceramic components;
wherein said bond comprises a glass-ceramic joining material and said ceramic components are joined by said joining material; and
wherein said ceramic components are composed of yttrium and/or scandium-stabilized zirconium oxide;
wherein said glass-ceramic joining material has a coefficient of thermal expansion α(20-300)≧9.5·10−6 K−1; and
wherein said glass-ceramic joining material, apart from at most impurities, is free of ZnO and free of PbO, and comprises, in mol% based on oxide content:
SiO2
3-<10
B2O3
16-34
Al2O3
7-15
CaO
8-40
BaO
25-38
MgO
0-10
ZrO2
0-5
Y2O3
0-10.

### Claim 5

An article comprising a bond between at least one metal component and at least one ceramic component;
wherein said bond comprises a glass-ceramic joining material and said at least one metal component and said at least one ceramic component are joined by said bondi
wherein said glass-ceramic joining material has a coefficient of thermal expansion α(20-300)≧9.5·10−6 K−1; and
wherein said glass-ceramic joining material, apart from at most impurities, is free of ZnO and free of PbO, and comprises, in mol% based on oxide content:
SiO2
3-<10
B2O3
16-34
Al2O3
7-15
CaO
8-40
BaO
25-38
MgO
0-10
ZrO2
0-5
Y2O3
0-10.

### Claim 6

An article comprising a bond between at least one metal component and at least one ceramic component;
wherein said bond comprises a glass-ceramic joining material and said at least one metal component and said at least one ceramic component are joined by said bond; and
wherein said at least one metal component is composed of ferritic stainless steel and said at least one ceramic component is composed of yttrium and/or scandium-stabilized zirconium oxide;
wherein said glass-ceramic joining material has a coefficient of thermal expansion α(20-300)≧9.5·10−6 K−1; and
wherein said glass-ceramic joining material, apart from at most impurities, is free of ZnO and free of PbO, and comprises, in mol% based on oxide content:
SiO2
3-<10
B2O3
16-34
Al2O3
7-15
CaO
8-40
BaO
25-38
MgO
0-10
ZrO2
0-5
Y2O3
0-10.

### Claim 7

A fuel cell comprising a glass-ceramic joining material having a coefficient of thermal expansion α(20-300)≧9.5·10−6 K−1, said glass-ceramic joining material comprising, in mol% based on oxide content:
SiO2
3-<10
B2O3
16-34
Al2O3
7-15
CaO
8-40
BaO
25-38
MgO
0-10
ZrO2
0-5
Y2O3
0-10.

### Claim 8

A method of producing a bond in a fuel cell, an electrolysis cell, a sensor or an actuator, said method comprising making said bond with a glass-ceramic joining material;
wherein said glass-ceramic joining material has a coefficient of thermal expansion α(20-300)≧9.5·10−6 K−1; and
wherein said glass-ceramic joining material, apart from at most impurities, is free of ZnO and free of PbO, and comprises, in mol% based on oxide content:
SiO2
3-<10
B2O3
16-34
Al2O3
7-15
CaO
8-40
BaO
25-38
MgO
0-10
ZrO2
0-5
Y2O3
0-10.