# US 8,278,376 B2 · Flame-retardant poly(arylene ether) composition and its use as a covering for coated wire

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 8,278,376 B2
- Document ID: US8278376B2
- Status: Granted
- Kind: B2
- Application number: 12/673,875
- Filed: 2008-09-05
- Published: 2011-11-03
- Granted: 2012-10-02
- Earliest claimed: 2008-09-05
- Assignees: Sabic Innovative Plastics IP B.V.
- Inventors: Weili Qiu; Jian Guo; Xiucuo Li; Hua Guo
- Web page: https://patentgrep.com/patent/US8278376B2

## CPC

- C08L 23/02: not modified by chemical after-treatment
- C08K 3/016: Flame-proofing or flame-retarding additives
- C08L 53/00: Compositions of block copolymers containing at least one sequence of a polymer obtained by reactions only involving carbon-to-carbon unsaturated bonds; Compositions of derivatives of such polymers
- C08L 53/02: of vinyl-aromatic monomers and conjugated dienes
- C08L 53/025: {modified}
- C08L 71/123: {not modified by chemical after-treatment}
- H01B 3/427: {Polyethers}
- H01B 3/441: {from alkenes}
- H01B 7/295: using material resistant to flame
- C08K 5/0091: {Complexes with metal-heteroatom-bonds}
- C08K 5/5313: Phosphinic compounds, e.g. R2=P(:O)OR'
- C08L 23/0815: {with aliphatic 1-olefins containing one carbon-to-carbon double bond}
- C08L 71/12: Polyphenylene oxides
- C08L 2201/02: Flame or fire retardant/resistant
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)
- H01B: CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES (selection for magnetic properties H01F1/00; waveguides H01P {; printed circuits H05K})

## Abstract

A flame retardant poly(arylene ether) composition is described. In addition to the poly(arylene ether), the composition includes a polyolefin component, and a flame retardant composition that includes a metal dialkyl phosphinate. The polyolefin component can be a polyolefin polymer and/or the polyolefin block of a poly(alkenyl aromatic)-polyolefin block copolymer. The composition is particularly suitable as a replacement for poly(vinyl chloride) in insulation for wire and cable.

## Claims

### Claim 1

A thermoplastic composition, comprising:
20 to 50 weight percent of a poly(arylene ether);
25 to 57 weight percent of total polyolefin; wherein total polyolefin consists of polyolefins and the polyolefin content of block copolymers comprising a poly(alkenyl aromatic) block and a polyolefin block; and
3 to 30 weight percent of a flame retardant composition comprising a metal dialkyl phosphinate;
wherein all weight percents are based on the total weight of the thermoplastic composition;
wherein the poly(arylene ether) and total polyolefin are present in a weight ratio of 0.53:1 to 1.2:1; and
wherein a test sample coated wire exhibits
a tensile stress at break of at least 10 megapascals, measured at 23° C. according to UL 1581, Section 470,
a tensile elongation at break of at least 100 percent, measured at 23° C. according to UL 1581, Section 470, and
a passing flame test rating according to UL 1581, Section 1080,
wherein the test sample coated wire consists of an AWG 24 conductor having a nominal cross sectional area of 0.205 millimeter2, and a tubular covering comprising the thermoplastic composition and having a nominal outer diameter of 2 millimeters.

### Claim 2 (depends on 1)

The thermoplastic composition of claim 1,
wherein the thermoplastic composition comprises 20 to 44 weight percent of the poly(arylene ether);
wherein the thermoplastic composition comprises 29 to 57 weight percent of total polyolefin;
wherein the thermoplastic composition comprises 10 to 25 weight percent of the flame retardant composition;
wherein the flame retardant composition comprises 1 to 10 weight percent of the metal dialkyl phosphinate; and
wherein the flame retardant composition further comprises
1 to 17 weight percent of a nitrogen-containing flame retardant selected from the group consisting of melamine phosphate, melamine pyrophosphate, melamine polyphosphates, and mixtures thereof, and
1 to 10 weight percent of a triaryl phosphate that is a liquid at one atmosphere and at least one temperature in the range 25 to 50° C.

### Claim 3 (depends on 2)

The thermoplastic composition of claim 2, wherein the test sample coated wire exhibits
a tensile stress at break of 10 to 30 megapascals, measured at 23° C. according to UL1581, Section 470, and
a tensile elongation at break of 100 to 240 percent, measured at 23° C. according to UL1581, Section 470.

### Claim 4 (depends on 2)

The thermoplastic composition of claim 2, wherein the test sample coated wire further exhibits a triaryl phosphate migration rating of 0, 1, or 2, measured as described in the working examples.

### Claim 5 (depends on 2)

The thermoplastic composition of claim 2, wherein the test sample coated wire further exhibits a heat deformation of 5 to 40 percent, measured at 121° C. and a 250 gram load according to UL 1581.

### Claim 6 (depends on 2)

The thermoplastic composition of claim 2, wherein the liquid triaryl phosphate represents 10 to 70 percent of the total weight of the flame retardant composition.

### Claim 7 (depends on 2)

The thermoplastic composition of claim 2, wherein the nitrogen-containing flame retardant and the metal dialkyl phosphate are present in a weight ratio of 0.5 to 8.

### Claim 8 (depends on 2)

The thermoplastic composition of claim 2, wherein the flame retardant composition consists of the metal dialkyl phosphinate, the nitrogen-containing flame retardant, and the liquid triaryl phosphate.

### Claim 9 (depends on 2)

The thermoplastic composition of claim 2, wherein the flame retardant composition further comprises 0.05 to 2.5 weight percent zinc borate.

### Claim 10 (depends on 2)

The thermoplastic composition of claim 2, further comprising 8 to 20 weight percent of total poly(alkenyl aromatic); wherein total poly(alkenyl aromatic) consists of poly(alkenyl aromatic)s and the poly(alkenyl aromatic) content of block copolymers comprising a poly(alkenyl aromatic) block and a polyolefin block.

### Claim 11 (depends on 2)

The thermoplastic composition of claim 2,
wherein the thermoplastic composition comprises 30 to 36 weight percent of the poly(arylene ether);
wherein the poly(arylene ether) is a poly(2,6-dimethyl-1,4-phenylene ether) having an intrinsic viscosity of 0.3 to 0.6 deciliter per gram measured in chloroform at 25° C.;
wherein the thermoplastic composition comprises 38 to 46 weight percent of total polyolefin weight percent of total polyolefin;
wherein the total polyolefin comprises polypropylene, ethylene-propylene copolymer, a poly(ethylene-co-propylene) block of a block copolymer comprising a polystyrene block and a poly(ethylene-co-propylene) block, and a poly(ethylene-co-butylene) block of a block copolymer comprising a polystyrene block and a poly(ethylene-co-butylene) block;
wherein the thermoplastic composition comprises 10 to 14 weight percent of the flame retardant composition consisting of
1 to 3 weight percent of aluminum tris(diethyl phosphinate),
1 to 3 weight percent of melamine polyphosphate, and
6 to 10 weight percent of bisphenol A bis(diphenyl phosphate);
wherein the poly(arylene ether) and total polyolefin are present in a weight ratio of 0.6 to 0.9; and
wherein the test sample coated wire exhibits
a tensile stress at break of 10 to 30 megapascals, measured at 23° C. according to UL1581, Section 470, and
a tensile elongation at break of 100 to 240 percent, measured at 23° C. according to UL1581, Section 470.

### Claim 12 (depends on 2)

The thermoplastic composition of claim 2,
wherein the thermoplastic composition exhibits
a UL 94 Vertical Burning Flame Test rating of V-0 or V-1 at a sample thickness less than or equal to 6.4 millimeters,
a tensile stress at break of at least 5 megapascals, measured at 23° C. according to ASTM D638, and
a flexural modulus of 10 to 1,000 megapascals, measured at 23° C. according to ASTM D790.

### Claim 13 (depends on 12)

The thermoplastic composition of claim 12,
wherein the UL 94 Vertical Burning Flame Test is conducted at a sample thickness of 3.0 to 6.4 millimeters, and
wherein the tensile stress at break is 5 to 21 megapascals.

### Claim 14 (depends on 2)

The thermoplastic composition of claim 2,
wherein the thermoplastic composition comprises 30 to 36 weight percent of the poly(arylene ether);
wherein the poly(arylene ether) is a poly(2,6-dimethyl-1,4-phenylene ether) having an intrinsic viscosity of 0.3 to 0.6 deciliter per gram measured in chloroform at 25° C.;
wherein the thermoplastic composition comprises 38 to 46 weight percent of total polyolefin weight percent of total polyolefin;
wherein the total polyolefin comprises polypropylene, ethylene-propylene copolymer, and a poly(ethylene-co-butylene) block of a block copolymer comprising a polystyrene block and a poly(ethylene-co-butylene) block;
wherein the thermoplastic composition comprises 10 to 14 weight percent of the flame retardant composition consisting of
1 to 3 weight percent of aluminum tris(diethyl phosphinate),
1 to 3 weight percent of melamine polyphosphate, and
6 to 10 weight percent of bisphenol A bis(diphenyl phosphate);
wherein the poly(arylene ether) and total polyolefin are present in a weight ratio of 0.6 to 0.9; and
wherein the thermoplastic composition exhibits
a UL 94 Vertical Burning Flame Test rating of V-0 or V-1 at a sample thickness of 6.4 millimeters,
a tensile stress at break of 12 to 21 megapascals, measured at 23° C. according to ASTM D638, and
a flexural modulus of 50 to 310 megapascals, measured at 23° C. according to ASTM D790.

### Claim 15 (depends on 1)

The thermoplastic composition of claim 1,
wherein the thermoplastic composition comprises 3 to 25 weight percent of the flame retardant composition;
wherein the flame retardant composition comprises 1 to 15 weight percent of the metal dialkyl phosphinate;
wherein the flame retardant composition further comprises 1 to 20 weight percent of a nitrogen-containing flame retardant selected from the group consisting of melamine phosphate, melamine pyrophosphate, melamine polyphosphates, and mixtures thereof;
wherein the poly(arylene ether) and total polyolefin are present in a weight ratio of 0.56:1 to 1.2:1; and
wherein the nitrogen-containing flame retardant and the metal dialkyl phosphinate are present in a ratio of 0.2:1 to 5:1.

### Claim 16 (depends on 15)

The thermoplastic composition of claim 15, wherein the flame retardant composition excludes triaryl phosphates that are liquids at one atmosphere and at least one temperature in the range 25 to 50° C.

### Claim 17 (depends on 16)

The thermoplastic composition of claim 16, wherein the test sample coated wire exhibits
a tensile stress at break of 10 to 30 megapascals, measured at 23° C. according to UL1581, Section 470, and
a tensile elongation at break of 100 to 350 percent, measured at 23° C. according to UL1581, Section 470.

### Claim 18 (depends on 16)

The thermoplastic composition of claim 16, wherein the test sample coated wire further exhibits a heat deformation of 5 to 50 percent, measured at 121° C. and a 250 gram load according to UL 1580.

### Claim 19 (depends on 16)

The thermoplastic composition of claim 16, wherein the flame retardant composition consists of the metal dialkyl phosphinate and the nitrogen-containing flame retardant.

### Claim 20 (depends on 16)

The thermoplastic composition of claim 16, wherein the flame retardant composition further comprises 0.05 to 2.5 weight percent zinc borate.

### Claim 21 (depends on 16)

The thermoplastic composition of claim 16, further comprising 3 to 20 weight percent of total poly(alkenyl aromatic); wherein total poly(alkenyl aromatic) consists of poly(alkenyl aromatic)s and the poly(alkenyl aromatic) content of block copolymers comprising a poly(alkenyl aromatic) block and a polyolefin block.

### Claim 22 (depends on 16)

The thermoplastic composition of claim 16,
wherein the thermoplastic composition comprises 37 to 47 weight percent of the poly(arylene ether);
wherein the poly(arylene ether) is a poly(2,6-dimethyl-1,4-phenylene ether) having an intrinsic viscosity of 0.3 to 0.6 deciliter per gram measured in chloroform at 25° C.;
wherein the thermoplastic composition comprises 34 to 43 weight percent of total polyolefin weight percent of total polyolefin;
wherein the total polyolefin comprises polypropylene, polybutene, ethylene-propylene copolymer, a poly(ethylene-co-propylene) block of a block copolymer comprising a polystyrene block and a poly(ethylene-co-propylene) block, and a poly(ethylene-co-butylene) block of a block copolymer comprising a polystyrene block and a poly(ethylene-co-butylene) block;
wherein the thermoplastic composition comprises 4 to 12 weight percent of the flame retardant composition consisting of
2 to 6 weight percent of aluminum tris(diethyl phosphinate), and
2 to 6 weight percent of melamine polyphosphate;
wherein the poly(arylene ether) and total polyolefin are present in a weight ratio of 0.8 to 1.2; and
wherein the test sample coated wire exhibits
a tensile stress at break of 10 to 25 megapascals, measured at 23° C. according to UL1581, Section 470, and
a tensile elongation at break of 200 to 300 percent, measured at 23° C. according to UL1581, Section 470.

### Claim 23 (depends on 16)

The thermoplastic composition of claim 16,
wherein the thermoplastic composition comprises 6 to 25 weight percent of the flame retardant composition;
wherein the poly(arylene ether) and total polyolefin are present in a weight ratio of 0.68:1 to 1.2:1;
wherein the metal dialkyl phosphinate and the nitrogen-containing flame retardant are present in a weight ratio of at least 5:1; and
wherein the thermoplastic composition exhibits
a UL 94 Vertical Burning Flame Test rating of V-0 or V-1 at a sample thickness less than or equal to 6.4 millimeters,
a tensile stress at break of at least 5 megapascals measured at 23° C. according to ASTM D638, and
a flexural modulus of 10 to 1,000 megapascals measured at 23° C. according to ASTM D790.

### Claim 24 (depends on 1)

The thermoplastic composition of claim 1,
wherein the flame retardant composition further comprises a triaryl phosphate that is a liquid at one atmosphere and at least one temperature in the range 25 to 50° C.; and
wherein the poly(arylene ether) and total polyolefin are present in a weight ratio of 0.55:1 to 1.2:1.

### Claim 25 (depends on 24)

The thermoplastic composition of claim 24, wherein the flame retardant composition excludes melamine phosphate, melamine pyrophosphate, and melamine polyphosphate.

### Claim 26 (depends on 25)

The thermoplastic composition of claim 25, wherein the test sample coated wire exhibits
a tensile stress at break of 10 to 25 megapascals, measured at 23° C. according to UL1581, Section 470, and
a tensile elongation at break of 100 to 360 percent, measured at 23° C. according to UL1581, Section 470.

### Claim 27 (depends on 25)

The thermoplastic composition of claim 25, wherein the test sample coated wire further exhibits a heat deformation of 5 to 20 percent, measured at 121° C. and a 250 gram load according to UL 1580.

### Claim 28 (depends on 25)

The thermoplastic composition of claim 25, further comprising 3 to 20 weight percent of total poly(alkenyl aromatic); wherein total poly(alkenyl aromatic) consists of poly(alkenyl aromatic)s and the poly(alkenyl aromatic) content of block copolymers comprising a poly(alkenyl aromatic) block and a polyolefin block.

### Claim 29 (depends on 25)

The thermoplastic composition of claim 25,
wherein the thermoplastic composition comprises 39 to 47 weight percent of the poly(arylene ether);
wherein the poly(arylene ether) is a poly(2,6-dimethyl-1,4-phenylene ether) having an intrinsic viscosity of 0.3 to 0.6 deciliter per gram measured in chloroform at 25° C.;
wherein the thermoplastic composition comprises 35 to 42 weight percent of total polyolefin weight percent of total polyolefin;
wherein the total polyolefin comprises polypropylene, polybutene, ethylene-propylene copolymer, a poly(ethylene-co-propylene) block of a block copolymer comprising a polystyrene block and a poly(ethylene-co-propylene) block, and a poly(ethylene-co-butylene) block of a block copolymer comprising a polystyrene block and a poly(ethylene-co-butylene) block;
wherein the thermoplastic composition comprises 4 to 10 weight percent of the flame retardant composition consisting of aluminum tris(diethyl phosphinate);
wherein the poly(arylene ether) and total polyolefin are present in a weight ratio of 0.9 to 1.2; and
wherein the test sample coated wire exhibits
a tensile stress at break of 10 to 25 megapascals, measured at 23° C. according to UL1581, Section 470, and
a tensile elongation at break of 150 to 300 percent, measured at 23° C. according to UL1581, Section 470.

### Claim 30 (depends on 1)

The thermoplastic composition of claim 1, wherein the flame retardant composition consists of the metal dialkyl phosphinate.

### Claim 31 (depends on 1)

An extruded article, comprising the product of extrusion molding the thermoplastic composition of claim 1.

### Claim 32 (depends on 1)

A coated wire, comprising:
a conductor, and
a covering disposed on the conductor;
wherein the covering comprises the thermoplastic composition of any of claim 1.