# US 8,277,872 B1 · Methods of making multi-scale carbon structures

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 8,277,872 B1
- Document ID: US8277872B1
- Status: Granted
- Kind: B1
- Application number: 12/617,617
- Filed: 2009-11-12
- Granted: 2012-10-02
- Earliest claimed: 2008-11-12
- Assignees: Stc.Unm
- Inventors: Marwan S. Al-Haik; Jonathan Phillips; Claudia Luhrs; Mahmoud Reda Taha
- Web page: https://patentgrep.com/patent/US8277872B1

## CPC

- C23C 16/26: Deposition of carbon only
- B82Y 30/00: Nanotechnology for materials or surface science, e.g. nanocomposites
- B82Y 40/00: Manufacture or treatment of nanostructures
- C01B 32/15: Nano-sized carbon materials
- C01B 32/16: Preparation
- C23C 16/0281: {of metallic sub-layers (C23C16/029 takes precedence)}
- C23C 18/08: characterised by the deposition of metallic material
- D01F 9/127: by thermal decomposition of hydrocarbon gases or vapours {or other carbon-containing compounds in the form of gas or vapour, e.g. carbon monoxide, alcohols}
- D01F 9/14: by decomposition of organic filaments
- D06M 11/74: with carbon or graphite; with carbides; with graphitic acids or their salts
- D06M 2101/28: Acrylonitrile; Methacrylonitrile
- D06M 2101/40: Fibres of carbon
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- B82Y: SPECIFIC USES OR APPLICATIONS OF NANOSTRUCTURES; MEASUREMENT OR ANALYSIS OF NANOSTRUCTURES; MANUFACTURE OR TREATMENT OF NANOSTRUCTURES
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- D01F: CHEMICAL FEATURES IN THE MANUFACTURE OF ARTIFICIAL FILAMENTS, THREADS, FIBRES, BRISTLES OR RIBBONS; APPARATUS SPECIALLY ADAPTED FOR THE MANUFACTURE OF CARBON FILAMENTS
- D06M: TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS

## Abstract

Methods of manufacturing a carbon structure including exposing a carbon fiber substrate to oxygen at a first predetermined temperature and activating the carbon fiber substrate by exposure to oxygen at a second predetermined temperature. A catalyst including palladium is deposited on the activated carbon fiber substrate. The deposited catalyst on the carbon fiber structure is exposed to a hydrocarbon at a third predetermined temperature to grow carbon structures thereon. The carbon structures grown can be multimodal in nature with structures that are nano-scale and/or submicron-scale.

## Claims

### Claim 1

A method of manufacturing a carbon structure comprising:
exposing a carbon fiber substrate to oxygen at a first predetermined temperature;
activating the carbon fiber substrate by exposure to oxygen at a second predetermined temperature;
depositing a catalyst on the activated carbon fiber substrate, wherein the catalyst comprises palladium; and
exposing the catalyst on the carbon fiber substrate to a hydrocarbon at a third predetermined temperature in order to grow a carbon structure thereon.

### Claim 2 (depends on 1)

The method of claim 1, further comprising rinsing the carbon fiber substrate with a solvent prior to the activating step.

### Claim 3 (depends on 1)

The method of claim 1, wherein the carbon fiber substrate comprises one of polyacrylonitrile fibers, pitch based carbon fibers, carbon nanofibers, carbon films, carbon foil, carbon fabric, carbon foam or carbon fiber bundles.

### Claim 4 (depends on 1)

The method of claim 1, wherein the first predetermined temperature is between 475 and 525 degrees Celsius.

### Claim 5 (depends on 4)

The method of claim 4, wherein the first predetermined temperature is approximately 500 degrees Celsius.

### Claim 6 (depends on 1)

The method of claim 1, wherein the second predetermined temperature is between 500 and 550 degrees Celsius.

### Claim 7 (depends on 6)

The method of claim 6, wherein the second predetermined temperature is approximately 525 degrees Celsius.

### Claim 8 (depends on 1)

The method of claim 1, wherein the third predetermined temperature is between 525 and 575 degrees Celsius.

### Claim 9 (depends on 8)

The method of claim 8, wherein the third predetermined temperature is approximately 550 degrees Celsius.

### Claim 10 (depends on 1)

The method of claim 1, wherein the first, second and third predetermined temperatures are less than 575 degrees Celsius.

### Claim 11 (depends on 1)

The method of claim 1, wherein the depositing step comprises administering an aqueous solution comprising palladium nitrate to the activated carbon fiber substrate.

### Claim 12 (depends on 11)

The method of claim 11, further comprising heating the carbon fiber substrate and the palladium nitrate to a fourth predetermined temperature in the presence of a hydrogen/nitrogen mixture to decompose the nitrate.

### Claim 13 (depends on 12)

The method of claim 12, wherein the fourth predetermined temperature is approximately 400 degrees Celsius.

### Claim 14 (depends on 12)

The method of claim 12, wherein the palladium comprises between 0.3 and 0.5% of the net weight of the carbon fiber substrate after the heating step at the fourth predetermined temperature.

### Claim 15 (depends on 1)

The method of claim 1, wherein exposing the catalyst on the carbon fiber substrate to a hydrocarbon at a third predetermined temperature comprises flowing a gas mixture comprising nitrogen, oxygen and one of acetylene, ethylene or methane, and the acetylene, ethylene or methane is a carbon source for growing the carbon structure.

### Claim 16 (depends on 15)

The method of claim 15, wherein the gas mixture comprises approximately 90% by volume N2, approximately 5% by volume O2, and approximately 5% by volume C2H4.

### Claim 17

A method for generating multiscale carbon-carbon structures, the method comprising:
exposing a polyacrylonitrile fiber substrate to oxygen at a temperature ranging between 475 and 525 degrees Celsius;
depositing a palladium catalyst on the polyacrylonitrile fiber substrate, the depositing comprising administering an aqueous solution comprising dissolved palladium nitrate to the polyacrylonitrile fiber substrate;
decomposing the nitrate thereby leaving substantially pure palladium particles as the palladium catalyst on the polyacrylonitrile fiber substrate;
and
exposing the palladium catalyst deposited on the polyacrylonitrile fiber substrate to a hydrocarbon at a temperature ranging between 525 and 575 degrees Celsius in order to grow a carbon structure thereon.

### Claim 18 (depends on 17)

The method of claim 17, wherein the substantially pure palladium particles are between 0.3 and 0.5% of the net weight of the polyacrylonitrile fiber substrate and wherein the palladium catalyst is exposed to the hydrocarbon by exposing the palladium catalyst to a gas mixture comprising of nitrogen, oxygen and one of acetylene, ethylene or methane.

### Claim 19

A method for generating multiscale carbon-carbon structures, the method comprising:
exposing a polyacrylonitrile fiber substrate to oxygen at a temperature ranging between 475 and 525 degrees Celsius;
rinsing the polyacrylonitrile fiber substrate in a solvent;
activating the polyacrylonitrile fiber substrate by exposure to oxygen at a temperature ranging between 500 and 550 degrees Celsius;
depositing a palladium catalyst on the activated polyacrylonitrile fiber substrate, the depositing comprising administering an aqueous solution comprising palladium nitrate to the activated polyacrylonitrile fiber substrate;
decomposing the nitrate thereby leaving, substantially pure palladium particles as the palladium catalyst on the polyacrylonitrile fiber substrate the substantially pure palladium particles are between 0.3% and 0.5% of the net weight of the polyacrylonitrile fiber substrate; and
exposing the substantially pure palladium particles on the polyacrylonitrile fiber substrate to a gas comprising ethylene at a temperature ranging between 525 and 575 degrees Celsius in order to grow a carbon structure thereon.