# US 8,277,772 B2 · Method of extracting Te and bismuth oxide and recovering byproducts

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 8,277,772 B2
- Document ID: US8277772B2
- Status: Granted
- Kind: B2
- Application number: 12/995,185
- Filed: 2009-06-02
- Published: 2011-03-31
- Granted: 2012-10-02
- Earliest claimed: 2008-06-02
- Assignees: Jun Wang
- Inventors: Jun Wang; Xiuzhen Wang; Zexian Song
- Web page: https://patentgrep.com/patent/US8277772B2

## CPC

- C01G 29/00: Compounds of bismuth
- C01B 19/02: Elemental selenium or tellurium
- C22B 3/08: Sulfuric acid {, other sulfurated acids or salts thereof}
- C22B 3/44: by chemical processes (treatment or purification of solutions by liquid-liquid extraction C22B3/26, by ion-exchange extraction C22B3/42)
- C22B 30/06: Obtaining bismuth
- C22B 61/00: Obtaining metals not elsewhere provided for in this subclass (iron C21)
- C01P 2006/80: Compositional purity
- Y02P 10/20: Recycling
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- C22B: PRODUCTION AND REFINING OF METALS (electrolytic C25); PRETREATMENT OF RAW MATERIALS
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A method of extracting Te and bismuth oxide and recovering byproduct comprises: leaching raw materials with a Te content of ≧1.8% by utilizing a leaching system containing H2SO4, Cl−, Br−, NH4+ and NaClO3, reducing leach solution with SO2 gas by precipitation method after separating impurities from it, washing with concentrated hydrochloric acid to obtain tellurium precipitation (18), purifying to obtain Te with a purity of higher than 99.99%. The filtrate produced is used for extracting Bi2O3 with a purity of higher than 99.99% when Bi content in the raw material is ≧2%. Acidic waste solution produced during the process could be returned to the leaching step for recycle.

## Claims

### Claim 1

A hydrometallurgical method for extracting tellurium, comprising the steps of material selecting, leaching the selected material, and reducing and purifying a leach solution, which is characterized in that:
the material selecting step includes selecting raw material with a tellurium content >1.8%; and
the leaching step includes:
placing the raw material in a leaching trough in which successively:
(1) a solution and/or solid containing Cl−, Br− and NH4+ is added at a ratio of Cl− >115 kg, Br− >16 kg and NH4+ >62 kg per ton of the raw material, with the liquid-solid ratio between the liquid and raw material in the leaching trough >1.5, and leaching at ambient temperature for 1 to 3 hours,
(2) then adding concentrated H2SO4 in an amount of 500 to 1000 kg per ton of raw material and leaching for 1 to 3 hours with leaching temperature being 45-65° C., and the residual acidity being 0.5 to 1.5 N,
(3) further adding NaClO3 in an amount of 25 to 50 kg of NaClO3 per ton of raw material, leaching under stirring for 2 hours or more with the leaching temperature being 75-95° C.;
filtering and washing, and then collecting the leach solution.

### Claim 2 (depends on 1)

The hydrometallurgical method for extracting tellurium according to claim 1, characterized in that the leaching step is followed by an impurity separation step comprising a precipitation process, wherein said impurity separation step includes: adjusting the pH of the leach solution to 2.7 to 3.1 a base bases, filtering and washing to obtain waste solution A and a precipitate, dissolving the precipitate with concentrated hydrochloric acid, filtering and then collecting filtrate which enters a reduction and purification step.

### Claim 3 (depends on 2)

The hydrometallurgical method for extracting tellurium according to claim 2, characterized in that:
the reduction step includes introducing sulfite or SO2 gas into the filtrate for reduction until Te <0.03 g/l, filtering and washing to obtain a tellurium-containing precipitate and filtrate B;
the purification step includes adding concentrated HCl in a liquid-solid ratio >1:1 into the above tellurium-containing precipitate for washing, filtering to obtain a tellurium precipitate and waste solution C, washing the tellurium precipitate with pure water until pH >3, filtering to obtain the tellurium precipitate and waste solution D, and baking the tellurium precipitate.

### Claim 4 (depends on 3)

The hydrometallurgical method for extracting tellurium according to claim 3, characterized in that the sulfite is Na2SO3.

### Claim 5 (depends on 3)

The hydrometallurgical method for extracting tellurium according to claim 3, wherein the method further includes returning the filtrate B from the reduction step back into part (1) of the leaching step for leaching or for extracting Bi2O3.

### Claim 6 (depends on 3)

The hvdrometallurgical method for according to claim 3, which further includes: adjusting the pH of the filtrate B with bases to 2.7-3.1, filtering and washing to obtain a bismuth-containing precipitate and waste solution E, transferring the bismuth-containing precipitate into an agitator with a pure water:solid ratio >1:1 and adding bases under stifling to adjust to pH 8-9, heating to 80-90° C., filtering and washing to obtain waste solution F and a Bi2O3 precipitate which is then baked.

### Claim 7 (depends on 6)

The hydrometallurgical method for according to claim 6, characterized in that the pH of the filtrate B is adjusted with bases to 2.9.

### Claim 8 (depends on 6)

The hydrometallurgical method for according to claim 6, characterized in that the base is NaOH and/or NH3.

### Claim 9 (depends on 6)

The hydrometallurgical method for according to claim 6, which further includes returning the waste solution E back into the step (1) of the leaching step for leaching.

### Claim 10 (depends on 6)

The hydrometallurgical method for according to claim 6, which further includes using the waste solution F for pH adjustment.

### Claim 11 (depends on 3)

The hydrometallurgical method for extracting tellurium according to claim 3, wherein the method further includes returning the waste solution C and/or waste solution D produced during the production processes back into part (1) of the leaching step for leaching.

### Claim 12 (depends on 3)

The hydrometallurgical method for extracting tellurium according to claim 3, wherein the method further includes returning and recycling the waste solution produced during the process for leaching so as to continuously increase the concentration of metals with trivial amount in the leach solution, and recovering when the concentration reaches the recovery condition.

### Claim 13 (depends on 2)

The hydrometallurgical method for extracting tellurium according to claim 2, characterized in that pH is adjusted to 2.9 by the base.

### Claim 14 (depends on 2)

The hydrometallurgical method for extracting tellurium according to claim 2, characterized in that the base is NaOH and/or NH3.

### Claim 15 (depends on 2)

The hydrometallurgical method for extracting tellurium according to claim 2, wherein the method further includes returning the waste solution A produced during the production processes back into part (1) of the leaching step for leaching.

### Claim 16 (depends on 2)

The hydrometallurgical method for extracting tellurium according to claim 2, wherein the method further includes returning and recycling the waste solution produced during the process for leaching so as to continuously increase the concentration of metals with trivial amount in the leach solution, and recovering when the concentration reaches the recovery condition.

### Claim 17 (depends on 1)

The hydrometallurgical method for extracting tellurium according to claim 1, characterized in that the solution and/or solid containing Cl−, Br− and NH4+ is a solution and/or solid of NH4Br and NH4Cl.

### Claim 18 (depends on 1)

The hydrometallurgical method for extracting tellurium according to claim 1, characterized in that the raw material is fine mineral powders of 80 meshes and above.