# US 8,277,710 B2 · Biaxially oriented hydrolysis-stable polyester film comprising epoxidized fatty acid derivatives, and process for production thereof and use thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 8,277,710 B2
- Document ID: US8277710B2
- Status: Granted
- Kind: B2
- Application number: 12/384,239
- Filed: 2009-04-02
- Published: 2010-05-13
- Granted: 2012-10-02
- Earliest claimed: 2008-11-11
- Assignees: Mitsubishi Polyester Film GmbH
- Inventors: Holger Kliesch; Dagmar Klein; Rainer Kurz; Dirk Broeder; Gottfried Hilkert; Volker Schaefer
- Web page: https://patentgrep.com/patent/US8277710B2

## CPC

- C08K 5/1515: Three-membered rings
- B29C 48/90: with calibration or sizing, i.e. combined with fixing or setting of the final dimensions of the extruded article
- B29C 48/91: Heating, e.g. for cross linking
- B29C 48/914: {Cooling drums}
- C08J 5/18: Manufacture of films or sheets
- C08L 67/02: Polyesters derived from dicarboxylic acids and dihydroxy compounds (C08L67/06 takes precedence)
- H01B 3/421: {Polyesters}
- H01G 4/18: of synthetic material, e.g. derivatives of cellulose (H01G4/16 takes precedence)
- B29C 48/906: {using roller calibration}
- C08J 2367/02: Polyesters derived from dicarboxylic acids and dihydroxy compounds; (C08J2367/06 takes precedence)
- C08L 91/00: Compositions of oils, fats or waxes; Compositions of derivatives thereof
- Y02A 40/966: Powered by renewable energy sources
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- C08J: WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H (working, e.g. shaping, of plastics B29)
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- H01B: CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES (selection for magnetic properties H01F1/00; waveguides H01P {; printed circuits H05K})
- H01G: CAPACITORS; CAPACITORS, RECTIFIERS, DETECTORS, SWITCHING DEVICES, LIGHT-SENSITIVE OR TEMPERATURE-SENSITIVE DEVICES OF THE ELECTROLYTIC TYPE (selection of specified materials as dielectric H01B3/00; capacitors having potential barriers H10D1/62, H10K10/10)
- Y02A: TECHNOLOGIES FOR ADAPTATION TO CLIMATE CHANGE

## Abstract

The invention relates to biaxially oriented polyester films which contain 0.1-5.0% by weight (based on the weight of the film) of a hydrolysis stabilizer based on epoxidized fatty acid esters and 0.2-10% by weight (based on the weight of the film) of epoxidized fatty acid glycerides, the epoxidized fatty acid esters having a mean molecular weight of at least 425 g/mol. Such films find use in outdoor applications, as a ribbon cable, as a backside laminate of solar modules and in electrical insulation applications.

## Claims

### Claim 1

A biaxially oriented polyester film comprising 0.1-5.0% by weight based on the weight of the film, of a hydrolysis stabilizer based on epoxidized fatty acid esters and 0.2-10% by weight, based on the weight of the film, of epoxidized fatty acid glycerides, said epoxidized fatty acid esters having a mean molecular weight of at least 425 g/mol, wherein more than 90% by weight of the epoxidized fatty acid esters are esters of the formula 2:
R4OR5 formula 2:
where R4 is defined as follows:
where RE =CH3 or H and
p =1-40
q =0-10
r 0-4
and the individual methylene (CH2)— (1), epoxy (CHOCH)— (2) and (CHCH3)— (3) groups may be present in any sequence and where
the R5 radical is described by the following formula 3:
—(CH2)S—R6 formula 3:
where s =0-50
R6=O—((CH2)u—O)v—Y where u =2-5, v =2-5000 and Y =H or CH3 or O—R4, where R4 corresponds to the R4 radical from formula 2.

### Claim 2 (depends on 1)

A biaxially oriented polyester film as claimed in claim 1 comprising 0.1-5.0% by weight, based on the weight of the film, of a hydrolysis stabilizer based on epoxidized fatty acid esters and 0.2-10% by weight, based on the weight of the film, of epoxidized fatty acid glycerides, said epoxidized fatty acid esters having a mean molecular weight of at least 425 g/mol.
wherein said film still has a standard viscosity based on DIN 53726 of more than 600 after 96 hours in an autoclave with steam saturation at 110° C.

### Claim 3 (depends on 1)

The polyester film as claimed in claim 1, wherein said film is white.

### Claim 4 (depends on 1)

The polyester film as claimed in claim 1, wherein said film comprises one or more additives selected from the group consisting of: inorganic particles, organic particles, flame retardants, free-radical scavengers, antioxidants and UV stabilizers.

### Claim 5 (depends on 4)

The polyester film as claimed in claim 4, wherein said film additionally comprises less than 5% by weight of further polymers.

### Claim 6 (depends on 1)

The polyester film as claimed in claim 1, wherein more than 80% by weight of the epoxidized fatty acid glycerides used are glyceryl esters of the formula 1
CH2OR1—CHOR2—CH2OR3 formula 1:
where the R1, R2 and R3 radicals are each independently defined as follows:
where RE=CH3 or H and
m=1-40
n=0-10
o=4
and the individual methylene (CH2)— (1), epoxy (CHOCH)— (2) and (CHCH3)— (3) groups may be present in any sequence,
and where R1,2,3 radicals where m=0 are present in glyceryl ester mixtures to an extent of less than 30% by weights, based on the total weight of the glyceryl esters.

### Claim 7 (depends on 6)

The polyester film as claimed in claim 6, wherein the fatty acid glycerides described by formula 1 are present in the overall hydrolysis stabilizer in an amount of greater than 40% by weight.

### Claim 8 (depends on 1)

The polyester film as claimed in claim 1, wherein more than 90% by weight of the epoxidized fatty acid esters are esters of the formula 2:
R4OR5 formula 2:
where R4 is defined as follows:
where RE=CH3 or H and
p=7-20
q=1-4
r=0.

### Claim 9 (depends on 8)

The polyester film as claimed in claim 8, wherein the fatty acid esters described by formula 2 are present in the overall hydrolysis stabilizer in an amount of greater than 5% by weight.

### Claim 10 (depends on 1)

The polyester film as claimed in claim 1, wherein the acid number of the hydrolysis stabilizers used is less than 10 mg KOH per gram, as determined pursuant to DIN EN ISO 3682.

### Claim 11 (depends on 1)

The polyester film as claimed in claim 1, wherein the epoxidized fatty acid esters and epoxidized fatty acid glycerides are present in a total amount of less than 10% by weight, based on the weight of the film.

### Claim 12 (depends on 1)

The polyester film as claimed in claim 1, wherein the epoxidized fatty acid esters and epoxidized fatty acid glycerides are present in a total amount of at least 1% by weight, based on the weight of the film.

### Claim 13 (depends on 1)

The polyester film as claimed in claim 1, wherein the epoxidized fatty acid esters have a mean number of epoxy groups per fatty acid ester molecule of less than 2 and/or greater than 1.5.

### Claim 14 (depends on 1)

The polyester film as claimed in claim 1, wherein the epoxidized fatty acid esters have a mean molecular weight of greater than 450 g/mol.

### Claim 15 (depends on 1)

The polyester film as claimed in claim 1, wherein the epoxidized fatty acid glyceride is selected from one or more epoxidized oils from the group consisting of: epoxidized soybean oil, epoxidized linseed oil, epoxidized colza oil, epoxidized sunflower oil and epoxidized fish oil.

### Claim 16 (depends on 1)

A process for producing a polyester film as claimed in claim 1, comprising
(i) extruding the melt compositions corresponding to the film through a flat die,
(ii) consolidating the film thus obtained by drawing the extruded melt off and quenching it on one or more chill rolls to form a substantially amorphous preliminary film,
(iii) orienting the substantially amorphous preliminary film by reheating and biaxially stretching the amorphous preliminary film and
(iv) heatsetting the biaxially stretched film and rolling the heatset film up,
wherein said film contains 0.1-5.0% by weights based on the weight of the film, of a hydrolysis stabilizer based on epoxidized fatty acid esters and 0.2-10% by weights, based on the weight of the film, of epoxidized fatty acid glycerides, said epoxidized fatty acid esters having a mean molecular weight of at least 425 g/mol.

### Claim 17 (depends on 1)

Outdoor film, ribbon cable, backside laminate of solar modules or electrical insulation comprising film as claimed in claim 1.

### Claim 18 (depends on 1)

A biaxially oriented polyester film as claimed in claim 1, wherein the total amount of the epoxidized fatty acid esters and the epoxidized fatty acid glycerides ranges from at least 1% to less than 10% by weight of the total weight of the film, and the resulting film has a modulus of elasticity in both directions of greater than 3000 N/mm2.

### Claim 19 (depends on 18)

A biaxially oriented polyester film as claimed in claim 18, wherein the total amount of the epoxidized fatty acid esters and the epoxidized fatty acid glycerides ranges from at least 1% to less than 7% by weight of the total weight of the film, the proportion of the fatty acid glycerides is greater than 40% by weight, based upon sum of the epoxidized fatty acid esters and the epoxidized fatty acid glycerides, the resulting film has a modulus of elasticity in both directions of greater than 4000 N/mm2and a density of greater than 1.3 g/cm3.

### Claim 20 (depends on 1)

A biaxially oriented polyester film as claimed in claim 1, wherein said film retains a higher amount of said epoxidized fatty acid ester in comparison to said film wherein the epoxidized fatty acid ester has a mean molecular weight of less than 425 g/mol.

### Claim 21 (depends on 1)

A biaxially oriented polyester film as claimed in claim 1, wherein said film exhibits lower outgassing, lower gelation and improved hyrdrolytic stability in comparison to said film wherein the epoxidized fatty acid ester has a mean molecular weight of less than 425 g/mol.

### Claim 22 (depends on 1)

A biaxially oriented polyester film as claimed in claim 1, wherein said hydrolysis stabilizer has a viscosity of greater than 300 mPa s at 25° C., per DIN 53018.

### Claim 23 (depends on 1)

A biaxially oriented polyester film as claimed in claim 1, wherein said film takes 30% longer in an autoclave with steam saturation at 110° C. to reach 400 standard viscosity units than an unstabilized polyester film.

### Claim 24 (depends on 1)

A biaxially oriented polyester film as claimed in claim 1, wherein R6 =O—R4 and said epoxidized fatty acid ester is a fatty acid diester.