# US 8,277,576 B2 · Steel material composition for producing piston rings and cylinder lines

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 8,277,576 B2
- Document ID: US8277576B2
- Status: Granted
- Kind: B2
- Application number: 13/203,596
- Filed: 2009-10-13
- Published: 2011-12-15
- Granted: 2012-10-02
- Earliest claimed: 2009-02-26
- Assignees: Federal-Mogul Burscheid GmbH
- Inventors: Laszlo Pelsoeczy
- Web page: https://patentgrep.com/patent/US8277576B2

## CPC

- C22C 38/38: with more than 1.5% by weight of manganese
- C21D 1/25: Hardening, combined with annealing between 300 degrees Celsius and 600 degrees Celsius, i.e. heat refining ("Vergüten")
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 9/08: for tubular bodies or pipes
- C21D 9/40: for rings; for bearing races
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

A steel material composition, in particular for producing piston rings and cylinder sleeves, contains the following elements in the cited fractions relative to 100% by weight of the steel material: 0.5-1.2% by weight C, 0-3.0% by weight Cr, 72.0-94.5% by weight Fe, 3.0-15.0% by weight Mn and 2.0-10.0% by weight Si. It can be produced by melting the starting materials and casting the melt into a pre-fabricated mold.

## Claims

### Claim 1

A piston ring, including a cast steel material composition as the basic element thereof, wherein the steel material composition consists of the following elements in the proportions indicated relative to 100% by weight of the steel material composition:
C:
0.5-1.2%
by weight
Cr:
0-3.0%
by weight
Fe:
72.0-94.5%
by weight
Mn:
3.0-15.0%
by weight
Si:
2.0-10.0%
by weight
Al:
max. 0.02%
by weight
B:
max. 0.1%
by weight
Cu:
max. 2.0%
by weight
Mo:
max. 3.0%
by weight
Nb:
max. 0.05%
by weight
Ni:
max. 4.0%
by weight
P:
max. 0.1%
by weight
S:
max. 0.05%
by weight
Sn:
max 0.05%
by weight
Ti:
max. 1.5%
by weight
V:
max. 1.5%
by weight
W:
max. 1.5%
by weight
wherein the sum of the fractions of Nb, Ti, V and W is not more than 1.5% by weight.

### Claim 2 (depends on 1)

The piston ring as recited in claim 1 wherein the steel material composition includes:
C:
0.5-0.7%
by weight, and
Mn:
5.05-15.0%
by weight.

### Claim 3

A method for producing a piston ring comprising
a. Producing a melt from a steel material composition consisting of
C:
0.5-1.2%
by weight
Cr:
0-3.0%
by weight
Fe:
72.0-94.5%
by weight
Mn:
3.0-15.0%
by weight
Si:
2.0-10.0%
by weight
Al:
max. 0.02%
by weight
B:
max. 0.1%
by weight
Cu:
max. 2.0%
by weight
Mo:
max. 3.0%
by weight
Nb:
max. 0.05%
by weight
Ni:
max. 4.0%
by weight
P:
max. 0.1%
by weight
S:
max. 0.05%
by weight
Sn:
max 0.05%
by weight
Ti:
max. 1.5%
by weight
V:
max. 1.5%
by weight
W:
max. 1.5%
by weight
wherein the sum of the fractions of Nb, Ti, V and W is not more than 1.5% by weight.

### Claim 4 (depends on 3)

The method of claim 3, further including:
c. Austenitising the piston ring above its Ac3 temperature,
d. Quenching the piston ring in a suitable quenching medium, and
e. Tempering the piston ring at a temperature in the range from 400 to 700° C. in a controlled atmosphere furnace.

### Claim 5 (depends on 4)

The method as recited in claim 4, wherein the production of the piston ring further includes the following step:
f. Nitriding the piston ring obtained.