# US 7,205,072 B2 · Layered cathode materials for lithium ion rechargeable batteries

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 7,205,072 B2
- Document ID: US7205072B2
- Status: Granted
- Kind: B2
- Application number: 10/699,484
- Filed: 2003-10-31
- Published: 2004-05-13
- Granted: 2007-04-17
- Earliest claimed: 2002-11-01
- Assignees: The University of Chicago
- Inventors: Sun-Ho Kang; Khalil Amine
- Web page: https://patentgrep.com/patent/US7205072B2

## CPC

- C01G 45/1228: of the type (MnO2)-, e.g. LiMnO2 or Li(MxMn1-x)O2
- C01G 53/42: containing alkali metals, e.g. LiNiO2
- C01G 53/502: containing lithium and cobalt
- H01M 4/131: Electrodes based on mixed oxides or hydroxides, or on mixtures of oxides or hydroxides, e.g. LiCoOx
- H01M 4/366: {as layered products}
- H01M 4/505: of mixed oxides or hydroxides containing manganese for inserting or intercalating light metals, e.g. LiMn2O4 or LiMn2OxFy
- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- H01M 4/582: {Halogenides}
- C01P 2002/20: Two-dimensional structures
- C01P 2002/54: one element only
- C01P 2002/72: by d-values or two theta-values, e.g. as X-ray diagram
- C01P 2004/02: obtained by optical microscopy
- C01P 2004/03: obtained by SEM
- C01P 2004/32: Spheres
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2004/80: Particles consisting of a mixture of two or more inorganic phases
- C01P 2006/40: Electric properties
- H01M 4/1315: containing halogen atoms, e.g. LiCoOxFy
- H01M 4/485: of mixed oxides or hydroxides for inserting or intercalating light metals, e.g. LiTi2O4 or LiTi2OxFy (H01M4/505, H01M4/525 take precedence)
- H01M 10/052: Li-accumulators
- Y02E 60/10: Energy storage using batteries
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

A number of materials with the composition Li1+xNiαMnβCoγM′δO2−zFz (M′=Mg,Zn,Al,Ga,B,Zr,Ti) for use with rechargeable batteries, wherein x is between about 0 and 0.3, α is between about 0.2 and 0.6, β is between about 0.2 and 0.6, γ is between about 0 and 0.3, δ is between about 0 and 0.15, and z is between about 0 and 0.2. Adding the above metal and fluorine dopants affects capacity, impedance, and stability of the layered oxide structure during electrochemical cycling.

## Claims

### Claim 1

A positive electrode material of substituted lithium nickel-manganese oxides for a non-aqueous lithium cell, comprising a composition of Li1+xNiαMnβCoγM′δO2−zXz wherein M′ is selected from the group consisting essentially of Mg, Zn, Al, Ga, B, Zr, and Ti, wherein X is selected from the group consisting essentially of F, Cl and I, wherein x is between a value greater than 0 and about 0.333, α is between about 0.2 and 0.6, β is between about 0.2 and 0.667, γ is between a value greater than 0 and about 0.333, δ is between a value greater than 0 and about 0.2, and z is between a value greater than 0 and about 0.5.

### Claim 2 (depends on 1)

The positive electrode material of claim 1, wherein the composition comprises Li1+xNiαMnβO2−zFz, and wherein x is between about a value greater than and about 0.333, α is between about 0.2 and 0.6, β is between about 0.2 and 0.667, and z is between about a value greater than 0 and about 0.5.

### Claim 3 (depends on 1)

The positive electrode material, of claim 1, wherein the composition comprises Li1+xNiαMnβCoγO2−zFz, and wherein x is between about a value greater than 0 and about 0.333, α is between about 0.2 and 0.6, β is between about 0.2 and 0.667, γ is between about 0.01 and 0.333, and z is between about a value greater than 0 and 0.5.

### Claim 4 (depends on 1)

The positive electrode material, of claim 1, wherein the composition comprises Li1+xNiαMnβAlδO2−zFz, and wherein x is between about a value greater than 0 and about 0.333, α is between about 0.2 and 0.6, β is between about 0.2 and 0.667, δ is between about 0.01 and 0.2, and z is between about a value greater than 0 and about 0.5.

### Claim 5 (depends on 1)

The positive electrode material of claim 1, wherein the composition comprises Li1−xNiαMnβTiδO2−zFz, wherein x is between about a value greater than 0 and about 0.333, α is between about 0.2 and 0.6, β is between about 0.2 and 0.667, δ is between about 0.01 and 0.2, and z is between about a value greater than 0 and about 0.5.

### Claim 6 (depends on 1)

The positive electrode material of claim 1, wherein the composition comprises Li1+xNiαMnβCoγAlδO2−zFz, and wherein x is between about a value greater than 0 and about 0.333, α is between about 0.2 and 0.6, β is between about 0.2 and 0.667, γ is between about 0.01 and 0.333, δ is between about 0.01 and 0.2, and z is between about a value greater than 0 and about 0.5.

### Claim 7 (depends on 1)

The positive electrode material of claim 1, wherein the composition comprises Li1+xNiαMnβCoγTiδO2−zFz, and wherein x is between about a value greater than 0 and about 0.333, α is between about 0.2 and 0.6, β is between about 0.2 and 0.667, γ is between about 0.01 and 0.333, δ is between about 0.01 and 0.2, and z is between about a value greater than 0 and about 0.5.

### Claim 8 (depends on 1)

The electrode material of claim 1, wherein the electrode material is formed by a solid state reaction process.

### Claim 9 (depends on 1)

The electrode material of claim 1, wherein the electrode material is formed by an aqueous solution based process.

### Claim 10 (depends on 1)

The electrode material of claim 1, wherein the electrode material is formed by a sol-gel process.

### Claim 11 (depends on 9)

The electrode material of claim 9, wherein the electrode material prepared by the steps of:
dissolving appropriate amounts of lithium hydroxide, lithium fluoride, nickel hydroxide, cobalt hydroxide, and M′-hydroxide or M′-nitrate; wherein M′ is selected from the group consisting essentially of Mg, Zn, Al, and Ga in distilled water whose pH was adjusted with nitric acid to form a first solution;
adding an aqueous solution of manganese acetate to the first solution to form a second solution;
refluxing the second solution in a flask attached with a condenser at about 80° C. for about 12–24 hours;
evaporating the second solution in a rotary vacuum evaporator to form a gel precursor;
eliminating organic contents from the gel precursor at about 400° C. for about 2 hours to form a powder; and
calcining the powder at about 900–1000° C. for about 10–24 hours in either an air or an oxygen containing atmosphere.

### Claim 12 (depends on 10)

The electrode material of claim 10, wherein the electrode material prepared by the steps of:
dissolving appropriate amounts of lithium acetate, lithium fluoride, nickel acetate, manganese acetate, cobalt acetate, and M′-acetate or M′-nitrate; wherein M′ is selected from the group consisting essentially of Mg, Zn, Al, and Ga in distilled water to form a first solution;
added the first solution to a glycolic/tartaric acid solution that is used as a chelating agent to form a second solution;
adjusting the pH of the second solution to about 7 using ammonium hydroxide, resulting in a gel precursor;
decomposing the gel precursor at about 4500 C for about 5 hours in air to form a decomposed power; and
firing the decomposed powder at about 900–1000° C. for about 10–24 hours in an air or an oxygen containing atmosphere,
wherein the dissolving, adding, and adjusting steps occur under continuous stirring and heating.

### Claim 13 (depends on 9)

The electrode material of claim 9, wherein the electrode material is prepared by the steps of:
mixing appropriate amounts of lithium hydroxide (or lithium carbonate), lithium fluoride, (Ni,Mn,Co)-hydroxide [or (Ni,Mn,Co)-carbonate], M′-hydroxide (or M′ oxide; wherein M′ is selected from the group consisting essentially of Mg, Zn, Al, Ga, B, Zr, and Ti);
calcined the mixed materials at about 450˜550° C. for about 12–30 hours in air; and calcining the mixed materials at about 900–1000° C. for about 10–24 hours either in air or in an oxygen-containing atmosphere.

### Claim 14

A non-aqueous lithium cell comprising:
a negative electrode;
a non-aqueous electrolyte; and
a positive electrode,
wherein the positive electrode has a composition of Li1+xNiaMnbCocM′δO2−zXz wherein M′ is selected from the group consisting essentially of Mg, Zn, Al, Ga, B, Zr, and Ti, wherein X is selected from the group consisting essentially of F, Cl and I, wherein x is between a value greater than 0 and about 0.333, α is between about 0.2 and 0.6, b is between about 0.2 and 0.667, c is between a value greater than 0 and about 0.333, δ is between a value greater than 0 and about 0.2, and z is between a value greater than 0 and about 0.5, and wherein oxidation states of Ni, Mn, and Co are Ni2+, Mn4+, and Co3+, respectively.

### Claim 15

A positive electrode material made of substituted lithium nickel-manganese oxides for non-aqueous lithium cell, comprising:
a composition of Li1+xNiαMnβCocM′δO2−zXz, wherein M′ is selected from the group consisting essentially of Mg, Zn, Al, Ga, B, Zr and Ti wherein X is selected from the group consisting essentially of F, Cl and I, wherein x, α, β, c, δ, and z are a value greater than 0 and are controlled so as to fix the oxidation states of Ni, Mn, and Co as Ni2+, Mn4+, and Co3+, respectively.

### Claim 16

A positive active material for a secondary lithium cell, comprising:
a core comprising at least one composition of Li1+xNiαMnβCoγM′δO2−zXz wherein M′ is selected from the group consisting essentially of Mg, Zn, Al, Ga, B, Zr, and Ti, wherein X is selected from the group consisting essentially of F, Cl and I, wherein x is between a value greater than 0 and about 0.333, α is between about 0.2 and 0.6, β is between about 0.2 and 0.667, γ is between a value greater than 0 and about 0.333, δ is between a value greater than 0 and about 0.2, and z is between a value greater than 0 and about 0.5; and
either a surface layer or a surface phase on the core, comprising at least one surface coating material from a coating material source selected from the group consisting of alkoxides, hydroxides, oxides and mixtures thereof,
wherein the surface-coated compound is heat-treated to form hydroxides or amorphous oxides on the compound surface.

### Claim 17 (depends on 16)

The positive active material of claim 16, wherein the amount of the surface coating material source is between about 0.05 and 10 percent by weight based upon the weight of the positive active material.

### Claim 18 (depends on 16)

The positive active material of claim 16, wherein the coating element of the surface coating material source comprises at least one element selected from the group consisting of Al, Bi, Ga, Ge, In, Mg, Pb, Si, Sn, Ti, Tl, Zn, Zr.

### Claim 19 (depends on 18)

The positive active material of claim 18, wherein the surface coating material source comprises Al-isopropoxide, zinc methoxide or indium-isopropoxide and is dissolved in ethanol.

### Claim 20 (depends on 16)

The positive active material of claim 16, wherein the heat-treating process is carried out at a temperature ranging from about 100 to 500° C. for a duration ranging from about 1 to 24 hours.