# US 6,730,354 B2 · Forming ferroelectric Pb(Zr,Ti)O3 films

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 6,730,354 B2
- Document ID: US6730354B2
- Status: Granted
- Kind: B2
- Application number: 09/925,223
- Filed: 2001-08-08
- Published: 2003-05-15
- Granted: 2004-05-04
- Earliest claimed: 2001-08-08
- Assignees: Agilent Technologies, Inc.; Applied Materials, Inc.; Texas Instruments Incorporated
- Inventors: Stephen R. Gilbert; Kaushal Singh; Sanjeev Aggarwal; Stevan Hunter
- Web page: https://patentgrep.com/patent/US6730354B2

## CPC

- H10P 14/69398: {the material having a perovskite structure, e.g. BaTiO3}
- C23C 16/409: {of the type ABO3 with A representing alkali, alkaline earth metal or lead and B representing a refractory metal, nickel, scandium or a lanthanide}
- H10P 14/668: {the materials being characterised by the deposition precursor materials}
- H10P 14/6334: {using decomposition or reaction of gaseous or vapour phase compounds, i.e. chemical vapour deposition (deposition by physical ablation of a target H10P14/6329)}
- Y10S 427/101: Liquid Source Chemical Depostion, i.e. LSCVD or Aerosol Chemical Vapor Deposition, i.e. ACVD
- H10P: GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- Y10S: TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS

## Abstract

Improved methods of forming PZT thin films that are compatible with industry-standard chemical vapor deposition production techniques are described. These methods enable PZT thin films having thicknesses of 70 nm or less to be fabricated with high within-wafer uniformity, high throughput and at a relatively low deposition temperature. In one aspect, a source reagent solution comprising a mixture of a lead precursor, a titanium precursor and a zirconium precursor in a solvent medium is provided. The source reagent solution is vaporized to form a precursor vapor. The precursor vapor is introduced into a chemical vapor deposition chamber containing the substrate. In another aspect, before deposition, the substrate is preheated during a preheating period. After the preheating period, the substrate is disposed on a heated susceptor during a heating period, after which a PZT film is formed on the heated substrate.

## Claims

### Claim 1

A method of forming a ferroelectric PZT film on a substrate, comprising:
metering from a source reagent ampoule a selected quantity of a premixed liquid source reagent solution comprising a mixture of a lead precursor, a titanium precursor and a zirconium precursor in a solvent medium;
vaporizing the metered source reagent solution to form a precursor vapor; and
introducing the precursor vapor into a chemical vapor deposition chamber containing the substrate.

### Claim 2 (depends on 1)

The method of claim 1, wherein the zirconium precursor comprises Zr(OiPr)2(thd)2 or Zr(thd)4 or Zr(OtBu)2(thd)2.

### Claim 3 (depends on 1)

The method of claim 1, wherein the lead precursor is Pb(thd)2(pmdeta), the zirconium precursor is Zr(OiPr)2(thd)2, and the titanium precursor is Ti(OiPr)2(thd)2.

### Claim 4 (depends on 1)

The method of claim 1, wherein the lead precursor, the titanium precursor and the zirconium precursor have a combined concentration between about 0.05 M and about 1.0 M in solution.

### Claim 5 (depends on 1)

The method of claim 1, wherein the source reagent solution is characterized by lead, zirconium and titanium concentrations between about 5% and 95%.

### Claim 6 (depends on 1)

The method of claim 1, further comprising introducing into the chemical vapor deposition chamber an oxidizing co-reactant gas comprising 5-100% N2O.

### Claim 7 (depends on 6)

The method of claim 6, wherein the oxidizing co-reactant gas comprises 50-75% N2O.

### Claim 8 (depends on 1)

The method of claim 1, further comprising introducing into the chemical vapor deposition chamber an oxidizing co-reactant gas comprising one or more of the following gases: N2O, O2, and O3.

### Claim 9 (depends on 1)

The method of claim 1, wherein the solvent medium comprises an octane-based solvent.

### Claim 10 (depends on 1)

The method of claim 1, wherein the source reagent solution is vaporized at a temperature in the range of about 180-210° C.

### Claim 11 (depends on 1)

The method of claim 1, further comprising maintaining the chemical vapor deposition chamber at a pressure in the range of about 0.5-10 torr during deposition.

### Claim 12 (depends on 11)

The method of claim 11, wherein the chemical vapor deposition chamber is maintained at a pressure in the range of about 0.5-4 torr during deposition.

### Claim 13 (depends on 12)

The method of claim 12, wherein the chemical vapor deposition chamber is maintained at a pressure of approximately 4 torr during deposition.

### Claim 14 (depends on 1)

The method of claim 1, wherein the source reagent solution is selected to obtain a precursor vapor having a Zr/(Zr+Ti) ratio in the range of about 0.05-0.70.

### Claim 15 (depends on 1)

The method of claim 1, wherein the source reagent solution is selected to obtain a precursor vapor having a Pb/(Zr+Ti) ratio in the range of about 0.3-3.0.

### Claim 16 (depends on 1)

The method of claim 1, further comprising preheating the substrate during a preheating period.

### Claim 17 (depends on 16)

The method of claim 16, wherein the preheating period is about 5-30 seconds long.

### Claim 18 (depends on 16)

The method of claim 16, further comprising disposing the preheated substrate on a heated susceptor during a heating period prior to formation of the PZT film on the substrate.

### Claim 19 (depends on 18)

The method of claim 18, wherein the heating period is about 30-60 seconds long or longer.

### Claim 20 (depends on 1)

The method of claim 1, further comprising providing a flow of a purge gas to reduce film depositions on susceptor and chamber wall surfaces.

### Claim 21

A method of forming a ferroelectric PZT film on a substrate, comprising:
providing a first premixed source reagent solution comprising a mixture of a lead precursor, a titanium precursor and a zirconium precursor in a solvent medium;
providing a second premixed source reagent solution comprising a second mixture of the lead precursor, the titanium precursor and the zirconium precursor in the solvent medium, wherein the first source reagent mixture is different from the second source reagent mixture;
mixing the first and second reagent solutions to form a precursor solution;
vaporizing the precursor solution to form a precursor vapor; and
introducing the precursor vapor into a chemical vapor deposition chamber containing the substrate.

### Claim 22 (depends on 21)

The method of claim 21, wherein the first and second source reagent solutions are characterized by a lead concentration in a range of about 28-65%, a zirconium concentration in a range of about 14-29%, and a titanium concentration in a range of about 20-43%.

### Claim 23

A method of forming a ferroelectric PZT film on a substrate, comprising:
introducing a substrate into a chemical vapor deposition chamber;
preheating the substrate during a preheating period;
after the preheating period, disposing the substrate on a heated susceptor during a heating period;
metering from a source reagent ampoule a selected quantity of a premixed liquid source reagent solution comprising a mixture of a lead precursor, a titanium precursor and a zirconium precursor in a solvent medium;
vaporizing the metered source reagent solution to form a precursor vapor; and
introducing the precursor vapor into the chemical vapor deposition chamber to form a ferroelectric PZT film on the heated substrate.

### Claim 24 (depends on 23)

The method of claim 23, wherein the substrate is preheated by supporting the substrate above the heated susceptor during the preheating period.

### Claim 25 (depends on 23)

The method of claim 23, further comprising providing a flow of a purge gas to reduce film depositions on susceptor and chamber wall surfaces.

### Claim 26

A method of forming a ferroelectric PZT film on a substrate, comprising:
introducing a substrate into a chemical vapor deposition chamber;
preheating the substrate during a preheating period;
after the preheating period, disposing the substrate on a heated susceptor during a heating period;
metering from a first liquid source a selected quantity of a first premixed liquid source reagent solution comprising a mixture of a lead precursor, a titanium precursor and a zirconium precursor in a solvent medium;
metering from a second liquid source a selected quantity of a second premixed liquid source reagent solution comprising a second mixture of the lead precursor, the titanium precursor and the zirconium precursor in the solvent medium, wherein the first source reagent mixture is different from the second source reagent mixture;
vaporizing the metered first and second source reagent solutions to form a precursor vapor; and
introducing the precursor vapor into the chemical vapor deposition chamber to form a ferroelectric PZT film on the heated substrate.

### Claim 27 (depends on 26)

The method of claim 26, further comprising mixing the first and second premixed liquid source reagent solutions to form a precursor mixture and, subsequently, vaporizing the precursor mixture to form the precursor vapor.

### Claim 28 (depends on 26)

The method of claim 26, wherein the first and second source reagent solutions are characterized by a lead concentration in a range of about 28-65%, a zirconium concentration in a range of about 14-29%, and a titanium concentration in a range of about 20-43%.