# US 6,458,218 B1 · Deposition and thermal diffusion of borides and carbides of refractory metals

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 6,458,218 B1
- Document ID: US6458218B1
- Status: Granted
- Kind: B1
- Application number: 09/759,299
- Filed: 2001-01-16
- Published: 2002-07-18
- Granted: 2002-10-01
- Earliest claimed: 2001-01-16
- Assignees: Linamar Corporation
- Inventors: Walter Savich
- Web page: https://patentgrep.com/patent/US6458218B1

## CPC

- C23C 8/02: Pretreatment of the material to be coated (C23C8/04 takes precedence)
- C23C 12/02: Diffusion in one step
- C25D 3/66: from melts
- C25D 5/50: by heat-treatment
- C25D 5/605: {Surface topography of the layers, e.g. rough, dendritic or nodular layers}
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR

## Abstract

A method is provided for depositing and thermally diffusing a boride or a carbide of a refractory metal on a substrate of a workpiece. A layer of the refractory metal is deposited on the substrate. At least one of the elements boron and carbon is deposited from a source other than the workpiece on the workpiece having the refractory metal layer. The workpiece is heated at a temperature and for a time period sufficient to diffuse at least a portion of the deposited refractory metal into the substrate and at least a portion of the deposited boron or carbon into the refractory metal layer and the substrate to form a substantially uniform and metallurgically bonded layer of the boride or carbide of the refractory metal on the substrate.

## Claims

### Claim 1

A method of providing a boride or carbide of a refractory metal on a substrate of a workpiece comprising the steps of:
(a) providing a first molten salt bath of an anhydrous fused salt electrolyte in an inert container, the molten salt lath comprising a substantially eutectic mixture of at least one halide from the group consisting of alkali metal halides and alkaline earth metal halides and a reducing agent for a refractory metal;
(b) immersing an anode comprising the refractory metal in the first molten salt bath;
(c) immersing a cathode comprising the workpiece in the first molten salt bath, the workpiece being electrically conductive;
(d) electrodepositing a layer of the refractory metal on the workpiece;
(e) heating the workpiece with the electrodeposited refractory metal thereon to a first temperature in a range of about 700° C. to about 900° C. for a first time period sufficient to diffuse at least a portion of the electrodeposited refractory metal into the substrate such that a refractory metal layer is metallurgically bonded to the substrate;
(f) providing a second molter salt bath in an inert crucible, the second molten salt bath comprising an anhydrous fused salt electrolyte comprising at least one halide from the group consisting of alkali metal halides and alkaline earth metal halides and a compound containing at least one second element from the group consisting of B and C;
(g) immersing the cathode comprising the workpiece having at least a portion of the electrodeposited refractory metal diffused therein in the second molten salt bath;
(h) electrodepositing a layer of the second element from the second molten bath on said workpiece having the refractory metal layer; and
(i) heating the workpiece having the second element electrodeposited on the layer of the refractory metal to a second temperature in the range of about 700° C. to about 900° C. for a second time period sufficient to diffuse at least a portion of the boron or carbon into the refractory metal layer and the substrate to form a boride or carbide of the refractory metal and to provide a substantially uniform and metallurgically bonded layer of the boride or carbide of the refractory metal on the substrate.

### Claim 2 (depends on 1)

A method as defined in claim 1 wherein the inert container contains a protective atmosphere of argon, for preventing contaminants from entering the container.

### Claim 3 (depends on 2)

A method as defined in claim 2 wherein the reducing agent is selected from the group consisting of a fluoride of the refractory metal and a chloride of the refractory metal.

### Claim 4 (depends on 3)

A method as defined in claim 3 wherein electrodepositing of the refractory metal is effected by passing direct current at a current density in the range of between about 5 mA per square centimeter to about 100 mA per square centimeter through the first molten salt bath between the anode and the cathode.

### Claim 5 (depends on 4)

A method as defined in claim 4 wherein electrodepositing of the second element is effected by passing direct current at a current density in the range of between about 200 mA per square centimeter to about 300 mA per square centimeter through the second molten salt bath.

### Claim 6 (depends on 5)

A method as defined in claim 5 wherein the refractory metal is selected from the group consisting of Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.

### Claim 7 (depends on 5)

A method as defined in claim 5 wherein the refractory metal is Nb.

### Claim 8 (depends on 7)

A method as defined in claim 7 wherein the second element is B and the second molten salt bath additionally comprises a second reducing agent for B.

### Claim 9 (depends on 8)

A method as defined in claim 8 wherein the first time period is between about five minutes and about three hours.

### Claim 10 (depends on 9)

A method as defined in claim 9 wherein the second temperature is about 800° C. and the second time period is between about one hour and about nine hours.

### Claim 11 (depends on 7)

A method as defined in claim 7 wherein the second element is C.

### Claim 12 (depends on 11)

A method as defined in claim 11 wherein the first time period is between about five minutes and about three hours.

### Claim 13 (depends on 12)

A method as defined in claim 12 wherein the electrodepositing of the C is effected by passing direct current through the second molten salt bath between the anode and the cathode at a current density of about 100 mA per square centimeter.

### Claim 14 (depends on 13)

A method as defined in claim 13 wherein the second temperature is about 750° C. and the second time period is about four hours.

### Claim 15 (depends on 5)

A. A method as defined in claim 5 wherein the refractory metal is Ta.

### Claim 16 (depends on 15)

A method as defined in claim 15 wherein the second element is B and the second molten salt bath additionally comprises potassium tetrafluoroborate.

### Claim 17 (depends on 16)

A method as defined in claim 16 wherein the first time period is between about five minutes and about three hours.

### Claim 18 (depends on 17)

A method as defined in claim 17 wherein the second temperature is about 900° C. and the second time period is about seven and one-half hours.

### Claim 19

A method of providing a carbide of a refractory metal on a substrate of a workpiece comprising the steps of:
(a) providing a first molten salt bath of an anhydrous fused salt electrolyte in an inert container, the molten salt lath comprising a substantially eutectic mixture of at least one halide from the group consisting of alkali metal halides and alkaline earth metal halides and a reducing agent for a refractory metal;
(b) immersing an anode comprising the refractory metal in the first molten salt bath;
(c) immersing a cathode comprising the workpiece in the first molten salt bath, the workpiece being electrically conductive;
(d) electrodepositing a layer of the refractory metal on the workpiece;
(e) heating the workpiece with the electrodeposited refractory metal thereon to a first temperature in a range of about 700° C. to about 900° C. for a first time period sufficient to diffuse at least a portion of the deposited refractory metal into the substrate such that a refractory metal layer is metallurgically bonded to the substrate;
(f) providing a second molten salt bath in an inert crucible, the second molten salt bath comprising a substantially eutectic mixture of at least one of the fluorides of Li, Na, or K, including a out two percent to about ten percent by weight the reducing agent of the refractory metal and about two percent to about ten percent by weight crystalline powder graphite;
(g) immersing the cathode comprising the workpiece having at least a portion of the electrodeposited refractory metal diffused therein in the second molten bath;
(h) electrodepositing a layer of carbon from the second molten salt bath on said workpiece having the refractory metal layer;
(i) heating the workpiece having the carbon electrodeposited on the layer of the refractory metal to a second temperature in the range of about 850° C. to about 900° C. for a second time period sufficient to diffuse at least a portion of the carbon into the refractory metal layer and the substrate to form a carbide of the refractory metal and to provide a substantially uniform and metallurgically bonded layer of the carbide of the refractory metal on the substrate.

### Claim 20 (depends on 19)

A method as defined in claim 19 wherein the refractory metal is Ta.

### Claim 21 (depends on 20)

A method as defined in claim 20 wherein the second molten salt bath comprises about five percent by weight potassium heptafluorotantalate and about five percent by weight crystalline powder graphite.

### Claim 22

A method of providing a carbide of a refractory metal on a substrate of a workpiece comprising the steps of:
(a) providing a first molten salt bath of an anhydrous fused salt electrolyte in an inert container, the molten salt bath comprising a substantially eutectic mixture of at least one halide from the group consisting of alkali metal halides and alkaline earth metal halides and a reducing agent for a refractory metal;
(b) immersing an anode comprising the refractory metal in the first molten salt bath;
(c) immersing a cathode comprising the workpiece in the first molten salt bath, the workpiece being electricaly conductive;
(d) electrodepositing a layer of the refractory metal on the workpiece;
(e) heating the workpiece with the electrodeposited refractory metal thereon to a first temperature in a range of about 700° C. to about 900° C. for a first time period sufficient to diffuse at least a portion of the electrodeposited refractory metal into the substrate such that a refractory metal layer is metallurgically bonded to the substrate;
(f) providing a crystalline graphite powder in an inert crucible;
(g) burying the workpiece having at least a portion of the electrodeposited refractory metal diffused therein in the crystalline graphite powder;
(h) compressing the crystalline graphite powder with pressure in the range of up to about 5,000 grams per square centimeter;
(i) evacuating air from the inert crucible;
(j) depositing a layer of car bon from the crystalline graphite powder on said workpiece having the refractory metal layer; and
(k) heating the workpiece to a second temperature in the range of about 1,000° C. to about 1,200° C. for a second time period sufficient to diffuse at least a portion of the carbon in the refractory metal layer and the substrate to form a carbide of the refractory metal and to provide a substantially uniform and metallurgically bonded layer of the carbide of the refractory metal on the substrate.

### Claim 23

A method of providing a carbide of a refractory metal on a substrate of a workpiece comprising the steps of:
(a) providing a first molten salt bath of an anhydrous fused salt electrolyte in an inert container, the molten salt bath comprising a substantially eutectic mixture of at least one halide from the group consisting of alkali metal halides and alkaline earth metal halides and a reducing agent for a refractory metal;
(b) immersing an anode comprising the refractory metal in the first molten salt bath;
(c) immersing a cathode comprising the workpiece in the first molten salt bath, the workpiece being electrically conductive;
(d) electrodepositing a layer of the refractory metal on the workpiece;
(e) heating the workpiece with the electrodeposited refractory metal thereon to a first temperature in a range of about 700° C. to about 900° C. for a first time period sufficient to diffuse at least a portion of the electro deposited refractory metal into the substrate such that a refractory metal layer is metallurgically bonded to the substrate;
(f) depositing a layer of carbon said workpiece having the refractory metal layer by gas carburizing; and
(g) heating the workpiece to a second temperature in the range of about 1,000° C. to about 1,400° C. for a second time period sufficient to diffuse at least a portion of the carbon in the refractory metal layer and the substrate to form a carbide of the refractory metal and to provide a substantially uniform and metallurgically bonded layer of the carbide of the refractory metal on the substrate.