A method for maintaining the sulfur level below 0.05% by weight, and preferably below 0.02% by weight, in the DRI product from the process for directly reducing ore containing iron oxides in a rotary kiln using a solid carbonaceous reducing agent, fed at the materials feed end and at the discharge end of the kiln, as both fuel and reductant is disclosed, identifying the important factors in the process affecting the sulfur levels in the DRI and steps and means for properly controlling these factors.
Claims7
In the process for directly reducing ore and other materials containing iron oxides in rotary kilns using a supply of sulfur-and-volatiles-containing solid carbonaceous materials as the sole source of both fuel and reductant, a portion of which supply is fed at the materials feed end of the kiln through which the process gases exhaust and the remaining portion of which supply is fed at the discharge end of the kiln through which the DRI product is discharged, and wherein a sulfur control agent is also fed to the kiln for removing sulfur from the feed materials, the improvement for achieving metallization of the DRI product consistently in the range from 90% to 95% while maintaining the sulfur level therein below 0.05% by weight comprising the steps of:
- using solid carbonaceous materials from said supply having less than 3% sulfur content;
- using iron-oxides-containing materials with a weight percent of sulfur less than 0.05%;
- screening the iron-oxides-containing materials fed to the kiln to eliminate particles thereof of a size less than about 1/8 inch;
- screening the sulfur control agent fed to the kiln to limit the size of its particles to less than about 1/8 inch;
- feeding the sulfur control agent at a rate in the range from 1% to 5% by weight of the iron-oxides-containing materials fed;
- maintaining the temperature of the process gases above the solids bed of materials in the region toward the feed end of the kiln above about 750.degree. C. to promote the removal of pyritic sulfur from said bed along with a proportion of the organic sulfur evolving from said bed with the volatiles from said carbonaceous materials;
- maintaining the temperature of the solids bed of materials in the region toward the discharge end of the kiln within the range of about 1070.+-.15.degree. C. to avoid sulfur absorption by the DRI product;
- maintaining the level of fixed carbon within the range of 5% to 15% by weight in the total materials discharged from the discharge end of the kiln;
- and
- returning to the kiln the charred reducing agent in the discharged materials from the kiln and screening out the sulfur control agent therefrom before returning said charred reducing agent to the kiln.