Process for the treatment of mineral slimes
AssigneeAmax Resource Recovery Systems, Inc.
InventorsArthur Raymond Mewes, Robert W. Styron, Mark Harris Smith
Life of this patent
Estimating the term…
Abstract
A method of dewatering mineral slimes by adding fly ash and then a polyelectrolyte and blending slowly and thoroughly. The clear water supernatant may be drawn off from the sedimented coagulated solids. The coagulated solids may be further dewatered or treated in ecologically beneficial ways.
Claims4
A method of dewatering about 5% phosphate slimes comprising adding ingredients consisting essentially of fly ash slurry and a low anionic polyacrylamide solution to said slime in the following manner:
- a. adding the fly ash slurry to the slime to be treated at a rate of approximately 0.2% by weight of total slime solution and thoroughly and gently mixing the resulting solution, followed relatively soon thereafter by the step of
- b. adding the polyacrylamide solution to the admixed fly ash and slime solution and thoroughly and gently mixing to initiate coagulation, said polyacrylamide having a concentration of approximately 0.002% and being added at the rate of 10-25% by weight of the total slime solution,
- c. allowing the coagulated solids to settle, and
- d. drawing off clear water separated from the coagulated solids on settling.
A method of dewatering about 5% phosphate slimes comprising adding ingredients consisting essentially of fly ash slurry and a low anionic polyacrylamide solution to said slime in the following manner:
- a. measuring the solids content of the slime to be treated,
- b. adjusting the slime content to approximately 5% or less solids by addition of make-up water as necessary to form a slime solution,
- c. pumping said slime solution into a mixing vessel so that said solution flows circularly in a clockwise direction,
- d. adding approximately 0.2% fly ash by weight of the total slime solution, said fly ash being in an aqueous slurry,
- e. gently and thoroughly mixing said fly ash into said slime solution,
- f. relatively soon thereafter adding approximately 10-25% by weight of the total slime solution of a low anionic polyacrylamide in aqueous solution at a 0.002% concentration,
- g. gently and thoroughly mixing said polyacrylamide into said slime solution and fly ash solution mixture to initiate coagulation,
- h. discharging said mixed solutions from said mixing vessel into a settling tank,
- i. allowing the coagulated solids to settle,
- j. discharging the coagulated solids into a holding pond for further processing, and
- k. drawing off clear water.
Dependencies are inferred from the claim text.