# US 2026/0312028 A1 · Cathode active material

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0312028 A1
- Document ID: US20260312028A1
- Status: Published application
- Kind: A1
- Application number: 19/463,620
- Filed: 2026-01-29
- Published: 2026-10-08
- Earliest claimed: 2025-04-02
- Assignees: Toyota Jidosha Kabushiki Kaisha
- Applicants: Toyota Jidosha Kabushiki Kaisha
- Inventors: Ryosuke OHSAWA
- Web page: https://patentgrep.com/patent/US20260312028A1

## CPC

- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- C01G 53/506: with the molar ratio of nickel with respect to all the metals other than alkali metals higher than or equal to 0.8, e.g. Li(MzNixCoyMn1-x-y-z)O2 with x ≥ 0.8
- C30B 29/22: Complex oxides
- C30B 30/04: using magnetic fields
- C01P 2006/40: Electric properties
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C30B: SINGLE-CRYSTAL GROWTH (by using ultra-high pressure, e.g. for the formation of diamonds, B01J3/06); UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL (zone-refining of metals or alloys C22B); PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE (casting of metals, casting of other substances by the same processes or devices B22D; working of plastics B29; modifying the physical structure of metals or alloys C21D, C22F); SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE (for producing semiconductor devices or parts thereof H10); APPARATUS THEREFOR
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS

## Abstract

The cathode active material includes at least one element selected from the group consisting of Ni, Co, and Mn. The cathode active material has a form in which two or more primary particles overlap each other. The primary particles are single crystals having a crystal structure belonging to space group R-3m. The primary particles are stacked such that the (003) planes of the primary particles are oriented parallel to each other. The ratio of the length of the shortest primary particle to the length of the longest primary particle among the primary particles, in a direction parallel to the (003) planes of the primary particles, is from 0.95 to 1.

## Claims

### Claim 1

A cathode active material comprising at least one element selected from the group consisting of Ni, Co, and Mn, wherein:
the cathode active material has a form in which two or more primary particles overlap each other;
the primary particles are single crystals having a crystal structure belonging to space group R-3m;
the primary particles are stacked such that (003) planes of the primary particles are oriented parallel to each other; and
a ratio of a length of a shortest primary particle to a length of a longest primary particle among the primary particles, in a direction parallel to the (003) planes of the primary particles, is from 0.95 to 1.

### Claim 2 (depends on 1)

The cathode active material according to claim 1, wherein:
the cathode active material has a form in which two to ten of the primary particles overlap each other;
the primary particles do not overlap each other in the direction parallel to the (003) planes of the primary particles; and
a short-axis direction of the cathode active material is parallel to the (003) planes of the primary particles.

### Claim 3 (depends on 1)

The cathode active material according to claim 1, wherein:
in an outer boundary of the cathode active material observed in a cross-sectional view obtained by a transmission electron microscope, the (003) planes derived from the primary particles are exposed at surfaces extending in the direction parallel to the (003) planes of the primary particles, and planes of the primary particles other than the (003) planes are exposed at surfaces extending in a direction perpendicular to the (003) planes of the primary particles; and
the planes of the primary particles other than the (003) planes are (012) planes, (101) planes, (104) planes, or (110) planes.

### Claim 4 (depends on 1)

A battery comprising a cathode layer containing the cathode active material according to claim 1.

### Claim 5 (depends on 1)

A method for producing the cathode active material according to claim 1, the method comprising:
performing first firing in which a first mixture of a transition metal hydroxide and a lithium compound is fired at 700° C. to 1100° C. to obtain a precursor of the cathode active material;
applying a magnetic field to a slurry in which the precursor of the cathode active material is dispersed in a solvent;
drying the slurry to obtain a dried product;
performing second firing in which the dried product is fired at 800° C. to 1000° C. to obtain a second-fired product; and
cooling the second-fired product at a cooling rate of 0.2° C./min to 0.5° C./min to obtain the cathode active material.