# US 2026/0312026 A1 · Cathode active material

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0312026 A1
- Document ID: US20260312026A1
- Status: Published application
- Kind: A1
- Application number: 19/461,985
- Filed: 2026-01-28
- Published: 2026-10-08
- Earliest claimed: 2025-04-02
- Assignees: Toyota Jidosha Kabushiki Kaisha
- Applicants: Toyota Jidosha Kabushiki Kaisha
- Inventors: Ryosuke OHSAWA
- Web page: https://patentgrep.com/patent/US20260312026A1

## CPC

- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- C01G 53/506: with the molar ratio of nickel with respect to all the metals other than alkali metals higher than or equal to 0.8, e.g. Li(MzNixCoyMn1-x-y-z)O2 with x ≥ 0.8
- C30B 29/22: Complex oxides
- C01P 2002/76: by a space-group or by other symmetry indications
- C01P 2004/04: obtained by TEM, STEM, STM or AFM
- C01P 2006/40: Electric properties
- H01M 2004/021: {Physical characteristics, e.g. porosity, surface area}
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C30B: SINGLE-CRYSTAL GROWTH (by using ultra-high pressure, e.g. for the formation of diamonds, B01J3/06); UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL (zone-refining of metals or alloys C22B); PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE (casting of metals, casting of other substances by the same processes or devices B22D; working of plastics B29; modifying the physical structure of metals or alloys C21D, C22F); SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE (for producing semiconductor devices or parts thereof H10); APPARATUS THEREFOR
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS

## Abstract

A cathode active material includes at least one element selected from the group consisting of Ni, Co, and Mn. The cathode active material has a form in which two or more primary particles overlap each other. The primary particles are single crystals having a crystal structure belonging to space group R-3m. The primary particles are stacked such that their (003) planes are oriented parallel to each other. In a cross-sectional view of the cathode active material obtained with a transmission electron microscope, the cathode active material has at least one first crack. The longitudinal direction of the first crack is parallel to the (003) planes of the primary particles.

## Claims

### Claim 1

A cathode active material comprising at least one element selected from the group consisting of Ni, Co, and Mn, wherein:
the cathode active material has a form in which two or more primary particles overlap each other;
the primary particles are single crystals having a crystal structure belonging to space group R-3m;
the primary particles are stacked such that (003) planes of the primary particles are oriented parallel to each other;
in a cross-sectional view of the cathode active material obtained with a transmission electron microscope, the cathode active material has at least one first crack; and
a longitudinal direction of the first crack is parallel to the (003) planes of the primary particles.

### Claim 2 (depends on 1)

The cathode active material according to claim 1, wherein:
in the cross-sectional view of the cathode active material obtained with the transmission electron microscope, the cathode active material has at least one second crack;
a longitudinal direction of the second crack is not parallel to the (003) planes of the primary particles; and
in the cross-sectional view of the cathode active material obtained with the transmission electron microscope, a ratio of a total longitudinal length of the first cracks to a sum of the total longitudinal length of the first cracks and a total longitudinal length of the second cracks is 15% or more.

### Claim 3 (depends on 1)

The cathode active material according to claim 1, wherein, in the cross-sectional view of the cathode active material obtained with the transmission electron microscope, a ratio of a longitudinal length of the first crack to a maximum diameter of the (003) plane of the primary particle is 10% or more.

### Claim 4 (depends on 1)

A battery comprising a cathode layer containing the cathode active material according to claim 1.

### Claim 5 (depends on 1)

A method for producing the cathode active material according to claim 1, the method comprising:
performing first firing in which a first mixture of a transition metal hydroxide and a lithium compound is fired at 700° C. to 1100° C. to obtain a precursor of the cathode active material;
applying a magnetic field to a slurry in which the precursor of the cathode active material is dispersed in a solvent;
drying the slurry to obtain a dried product;
performing second firing in which the dried product is fired at 800° C. to 1000° C. to obtain a fired product; and
pressing the fired product at a predetermined pressure in a direction perpendicular to an orientation direction of the magnetic field to obtain the cathode active material.