# US 2026/0312009 A1 · Negative electrode material and preparation method thereof, battery, and electrical device

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0312009 A1
- Document ID: US20260312009A1
- Status: Published application
- Kind: A1
- Application number: 19/176,165
- Filed: 2025-04-11
- Published: 2026-10-08
- Earliest claimed: 2023-01-03
- Assignees: Contemporary Amperex Technology (Hong Kong) Limited
- Applicants: Contemporary Amperex Technology (Hong Kong) Limited
- Inventors: Kai WU; Liangbin LIU; Jiazheng WANG; Yuwei QIN; Jingxian DENG; Zijian LV; Xiaobin DONG; Yuan LI
- Web page: https://patentgrep.com/patent/US20260312009A1

## CPC

- H01M 4/366: {as layered products}
- C01B 32/05: Preparation or purification of carbon not covered by groups C01B32/15, C01B32/20, C01B32/25, C01B32/30
- H01M 4/5815: {Sulfides}
- H01M 4/587: for inserting or intercalating light metals
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- B60L 50/64: Constructional details of batteries specially adapted for electric vehicles
- B60R 16/033: characterised by the use of electrical cells or batteries (for propulsion puposes B60K1/04; supplying batteries to, or removing batteries from, vehicles B60S5/06; testing of charge state G01R31/36)
- C01P 2002/52: containing elements as dopants
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2004/64: Nanometer sized, i.e. from 1-100 nanometer
- C01P 2004/84: one phase coated with the other
- C01P 2006/12: Surface area
- C01P 2006/14: Pore volume
- C01P 2006/17: Pore diameter distribution
- C01P 2006/40: Electric properties
- H01M 2220/20: Batteries in motive systems, e.g. vehicle, ship, plane
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- B60L: PROPULSION OF ELECTRICALLY-PROPELLED VEHICLES (arrangements or mounting of electrical propulsion units or of plural diverse prime-movers for mutual or common propulsion in vehicles B60K1/00, B60K6/20; arrangements or mounting of electrical gearing in vehicles B60K17/12, B60K17/14; preventing wheel slip by reducing power in rail vehicles B61C15/08; dynamo-electric machines H02K; control or regulation of electric motors H02P); SUPPLYING ELECTRIC POWER FOR AUXILIARY EQUIPMENT OF ELECTRICALLY-PROPELLED VEHICLES (electric coupling devices combined with mechanical couplings of vehicles B60D1/64; electric heating for vehicles B60H1/00); ELECTRODYNAMIC BRAKE SYSTEMS FOR VEHICLES IN GENERAL (control or regulation of electric motors H02P); MAGNETIC SUSPENSION OR LEVITATION FOR VEHICLES; MONITORING OPERATING VARIABLES OF ELECTRICALLY-PROPELLED VEHICLES; ELECTRIC SAFETY DEVICES FOR ELECTRICALLY-PROPELLED VEHICLES
- B60R: VEHICLES, VEHICLE FITTINGS, OR VEHICLE PARTS, NOT OTHERWISE PROVIDED FOR
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS

## Abstract

This application discloses a negative electrode material and a preparation method thereof, a battery, and an electrical device. The negative electrode material includes porous carbon. The porous carbon includes iron and/or sulfur. An active material is included in pores of the porous carbon. In this way, this application endows the negative electrode material with high conductivity, small volume expansion, and high surface activity, thereby endowing the battery with a high capacity and excellent C-rate performance and cycle performance.

## Claims

### Claim 1

A negative electrode material, characterized in that the negative electrode material comprises porous carbon, the porous carbon comprises iron and/or sulfur, and an active material is comprised in pores of the porous carbon.

### Claim 2 (depends on 1)

The negative electrode material according to claim 1, characterized in that
a content of iron in the negative electrode material is 50 to 3000 ppm; and/or
a content of sulfur in the negative electrode material is 100 to 1500 ppm.

### Claim 3 (depends on 1)

The negative electrode material according to claim 1, characterized in that an average pore diameter of the porous carbon is 2 to 50 nm.

### Claim 4 (depends on 1)

The negative electrode material according to claim 1, characterized in that a pore volume of the porous carbon is 0.1 to 2.0 cm3/g.

### Claim 5 (depends on 1)

The negative electrode material according to claim 1, characterized in that a content ratio between micropores, mesopores, and macropores in the porous carbon is (5% to 25%):(65% to 90%):(5% to 15%).

### Claim 6 (depends on 1)

The negative electrode material according to claim 1, wherein the active material comprises a silicon-carbon material, and the silicon-carbon material comprises silicon nanoparticles and carbon nanoparticles.

### Claim 7 (depends on 6)

The negative electrode material according to claim 6, characterized in that
a particle diameter of the silicon nanoparticles is less than or equal to 10 nm; and/or
a particle diameter of the carbon nanoparticles is less than or equal to 30 nm.

### Claim 8 (depends on 6)

The negative electrode material according to claim 6, characterized in that a mass ratio of silicon to carbon in the negative electrode material is Si:C=(20 to 55):(40 to 75).

### Claim 9 (depends on 6)

The negative electrode material according to claim 6, characterized in that a mass ratio between silicon, carbon, and oxygen in the negative electrode material is Si:C:O=(20 to 55):(40 to 75):(0.5 to 5).

### Claim 10 (depends on 1)

The negative electrode material according to claim 1, characterized in that
a particle diameter Dv50 of the negative electrode material is 3 to 8 μm; and/or
a porosity of the negative electrode material is 5% to 30%; and/or
a specific surface area of the negative electrode material is less than or equal to 5.0 m2/g.

### Claim 11 (depends on 1)

A battery, characterized in that the battery comprises a positive electrode plate, a separator, and a negative electrode plate, the separator is located between the positive electrode plate and the negative electrode plate to serve a separation function, the negative electrode plate comprises a negative electrode material and a negative current collector, and the negative electrode material comprises the negative electrode material according to claim 1.

### Claim 12 (depends on 11)

An electrical device, characterized in that the electrical device comprises the battery according to claim 11.

### Claim 13 (depends on 1)

A method for preparing a negative electrode material, characterized in that the method comprises:
providing a porous carbon precursor, wherein the porous carbon precursor comprises a carbon precursor, an iron precursor, and/or a sulfur precursor;
treating the porous carbon precursor to obtain porous carbon; and
depositing an active material in pores of the porous carbon to obtain the negative electrode material according to claim 1.

### Claim 14 (depends on 13)

The method for preparing a negative electrode material according to claim 13, characterized in that
the iron precursor comprises one or more of ferric trichloride, ferric nitrate, ferric sulfate, carbonyl iron, or ferrocene; and/or
the sulfur precursor comprises one or more of hydrogen sulfide (H2S), thiophene, a thiophene compound, thiol, thiophenol, or thioether.

### Claim 15 (depends on 13)

The method for preparing a negative electrode material according to claim 13, characterized in that the depositing an active material in pores of the porous carbon comprises:
depositing the active material in the pores of the porous carbon by gas phase co-deposition to form silicon nanoparticles and carbon nanoparticles.

### Claim 16 (depends on 15)

The method for preparing a negative electrode material according to claim 15, characterized in that
a volume ratio of a silicon source gas to a carbon source gas for silicon-carbon co-deposition is greater than or equal to 6:1; and/or
a concentration of a silicon source gas in a gas source for silicon-carbon co-deposition is 5% to 80%.

### Claim 17 (depends on 15)

The method for preparing a negative electrode material according to claim 15, characterized in that
a silicon source gas for the co-deposition comprises one or more of monosilane, disilane, trisilane, monochlorosilane, dichlorosilane, or trichlorosilane; and/or
a carbon source gas for the co-deposition comprises one or more of methane, ethane, butane, propane, ethylene, propylene, butene, or acetylene.

### Claim 18 (depends on 13)

The method for preparing a negative electrode material according to claim 13, characterized in that the method further comprises:
performing gas phase deposition on the porous carbon to form a carbon coating layer, wherein
a deposition gas for the gas phase deposition is a mixed gas of C2H2 and N2, wherein a volume percent of C2H2 is 2% to 20%, a gas flow rate introduced is 100 to 300 mL/min, a reaction temperature is 800° C. to 1000° C., and a deposition reaction time is 0.5 to 2 hours.