# US 2026/0297708 A1 · Aluminum alloy sheet and method for producing aluminum alloy sheet

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0297708 A1
- Document ID: US20260297708A1
- Status: Published application
- Kind: A1
- Application number: 19/576,578
- Filed: 2026-03-24
- Published: 2026-10-01
- Earliest claimed: 2025-03-31
- Assignees: Kabushiki Kaisha Kobe Seiko Sho (Kobe Steel, Ltd.)
- Applicants: Kabushiki Kaisha Kobe Seiko Sho (Kobe Steel, Ltd.)
- Inventors: Masato ISHIHARA; Takahiro HASHIMOTO
- Web page: https://patentgrep.com/patent/US20260297708A1

## CPC

- C22C 21/02: with silicon as the next major constituent
- B22D 21/007: {with low melting point, e.g. Al 659 degrees C, Mg 650 degrees C}
- C22F 1/002: {by rapid cooling or quenching; cooling agents used therefor}
- C22F 1/043: of alloys with silicon as the next major constituent
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

An aluminum alloy sheet includes, by mass %, 0.3% to 1.5% of Si, 0.15% to 0.4% of Fe, 0.001% to 0.2% of Cu, 0.02% to 0.3% of Mn, 0.3% to 0.8% of Mg, 0.001% to 0.3% of Cr, 0.001% to 0.3% of Zn, and 0.001% to 0.3% of Ti with the remainder being Al and impurities. The aluminum alloy sheet has an area fraction of Cube orientation of 17% to 50%. A number density of Mg—Si-based compounds having an equivalent circle diameter of 0.4 μm or more in the aluminum alloy sheet is 2650 particles/mm2 or less, and a number density of Al—Fe—Si-based compounds having an equivalent circle diameter of 2.0 μm or more in the aluminum alloy sheet is 225 particles/mm2 to 700 particles/mm2.

## Claims

### Claim 1

An aluminum alloy sheet comprising:
0.3 mass % to 1.5 mass % of Si;
0.15 mass % to 0.4 mass % of Fe;
0.001 mass % to 0.2 mass % of Cu;
0.02 mass % to 0.3 mass % of Mn;
0.3 mass % to 0.8 mass % of Mg;
0.001 mass % to 0.3 mass % of Cr;
0.001 mass % to 0.3 mass % of Zn; and
0.001 mass % to 0.3 mass % of Ti,
with the remainder being Al and impurities, wherein
the aluminum alloy sheet has an area fraction of Cube orientation of 17% to 50%,
a number density of Mg—Si-based compounds having an equivalent circle diameter of 0.4 μm or more in the aluminum alloy sheet is 2650 particles/mm2 or less, and
a number density of Al—Fe—Si-based compounds having an equivalent circle diameter of 2.0 μm or more in the aluminum alloy sheet is 225 particles/mm2 to 700 particles/mm2.

### Claim 2

A method for producing an aluminum alloy sheet, the method comprising: in the following order,
a casting step of melting raw materials to obtain a molten metal having a predetermined chemical composition and casting the molten metal into a slab;
a homogenization heat treatment step of subjecting the cast slab to a homogenization heat treatment;
a hot rough rolling step of subjecting the homogenized slab to hot rough rolling to obtain a hot rough rolled sheet;
a hot finish rolling step of subjecting the hot rough rolled sheet to hot finish rolling to obtain a hot finish rolled sheet;
a cold rolling step of subjecting the hot finish rolled sheet to cold rolling to obtain a cold rolled sheet; and
a solution treatment step of subjecting the cold rolled sheet to a solution treatment, wherein
in the homogenization heat treatment step, the homogenization heat treatment is performed in a temperature range of 520° C. to 580° C.,
no cooling and no additional heat treatment are performed between the homogenization heat treatment step and the hot rough rolling step,
in the hot rough rolling step, a final pass is performed under a condition that a Z factor, as expressed by the following formula, is 1.0×108 to 5.0×1011,
Z
=
ε
.
⁢
exp
⁡
(
Q
/
RT
)
wherein ε′ represents a strain rate, Q represents activation energy, R represents a gas constant, and T represents a temperature,
the hot finish rolling step is performed such that an end temperature is 250° C. or higher and lower than 350° C.,
the cold rolling step is performed such that a cold rolling ratio is 74% to 95%, and
the obtained aluminum alloy sheet contains
0.3 mass % to 1.5 mass % of Si,
0.15 mass % to 0.4 mass % of Fe,
0.001 mass % to 0.2 mass % of Cu,
0.02 mass % to 0.3 mass % of Mn,
0.3 mass % to 0.8 mass % of Mg,
0.001 mass % to 0.3 mass % of Cr,
0.001 mass % to 0.3 mass % of Zn, and
0.001 mass % to 0.3 mass % of Ti,
with the remainder being Al and impurities.

### Claim 3 (depends on 2)

The method according to claim 2, wherein
the homogenization heat treatment step is performed for 1 hour to 30 hours.

### Claim 4 (depends on 2)

The method according to claim 2, wherein
the hot rough rolling step is performed such that an entry temperature is 400° C. to 570° C.

### Claim 5 (depends on 3)

The method according to claim 3, wherein
the hot rough rolling step is performed such that an entry temperature is 400° C. to 570° C.

### Claim 6 (depends on 2)

The method according to claim 2, further comprising:
a step of performing intermediate annealing before the cold rolling step or during the cold rolling step.

### Claim 7 (depends on 3)

The method according to claim 3, further comprising:
a step of performing intermediate annealing before the cold rolling step or during the cold rolling step.

### Claim 8 (depends on 6)

The method according to claim 6, wherein
the intermediate annealing is performed in a temperature range of 300° C. to 450° C. for 1 hour to 20 hours.

### Claim 9 (depends on 7)

The method according to claim 7, wherein
the intermediate annealing is performed in a temperature range of 300° C. to 450° C. for 1 hour to 20 hours.

### Claim 10 (depends on 2)

The method according to claim 2, wherein
the solution treatment step is performed in a temperature range of 520° C. to 580° C.

### Claim 11 (depends on 3)

The method according to claim 3, wherein
the solution treatment step is performed in a temperature range of 520° C. to 580° C.

### Claim 12 (depends on 2)

The method according to claim 2, wherein
cooling is performed at a cooling rate of 1° C./sec to 100° C./sec after the solution treatment.

### Claim 13 (depends on 3)

The method according to claim 3, wherein
cooling is performed at a cooling rate of 1° C./sec to 100° C./sec after the solution treatment.

### Claim 14 (depends on 2)

The method according to claim 2, wherein
a preliminary aging treatment is performed by holding the sheet at a temperature in a range of 50° C. to 100° C. for 1 hour to 50 hours within 10 minutes after the solution treatment step.

### Claim 15 (depends on 3)

The method according to claim 3, wherein
a preliminary aging treatment is performed by holding the sheet at a temperature in a range of 50° C. to 100° C. for 1 hour to 50 hours within 10 minutes after the solution treatment step.