# US 2026/0297707 A1 · High-strength and low-modulus antibacterial alloy, preparation method therefor, and use thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0297707 A1
- Document ID: US20260297707A1
- Status: Published application
- Kind: A1
- Application number: 19/309,830
- Filed: 2025-08-26
- Published: 2026-10-01
- Earliest claimed: 2025-03-25
- Assignees: Dongfang Jiayue(Jiangsu) Medical Technology Company Ltd.
- Applicants: Dongfang Jiayue(Jiangsu) Medical Technology Company Ltd.
- Inventors: LU WANG; TAO ZHANG; JING RUAN; MEIJUN JIANG
- Web page: https://patentgrep.com/patent/US20260297707A1

## CPC

- C22C 14/00: Alloys based on titanium
- A61K 6/84: comprising metals or alloys
- A61P 31/04: Antibacterial agents
- B05D 1/18: performed by dipping
- C22C 1/1036: {starting from a melt}
- C22F 1/183: {of titanium or alloys based thereon}
- B05D 2202/35: based on Ti
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- A61K: PREPARATIONS FOR MEDICAL, DENTAL OR TOILETRY PURPOSES (devices or methods specially adapted for bringing pharmaceutical products into particular physical or administering forms A61J3/00; chemical aspects of, or use of materials for deodorisation of air, for disinfection or sterilisation, or for bandages, dressings, absorbent pads or surgical articles A61L; soap compositions C11D)
- A61P: SPECIFIC THERAPEUTIC ACTIVITY OF CHEMICAL COMPOUNDS OR MEDICINAL PREPARATIONS
- B05D: PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL (conveying articles or workpieces through baths of liquid B65G, e.g. B65G49/02)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

Disclosed are a high-strength and low-modulus antibacterial alloy, a preparation method therefor, and use thereof. The high-strength and low-modulus antibacterial alloy has a molecular formula of TiaZrbNbcCudAgeOf, where subscripts a, b, c, d, e, and f represent atomic percentages of corresponding alloy elements, with 50≤a≤70, 20≤b≤30, 5≤c≤7, 2≤d≤4, 1≤e≤5, 2≤f≤4, and a+b+c+d+e+f=100; and a remainder is an unavoidable impurity. Through component optimization and process innovation, a microstructure of the alloy is effectively controlled, thereby significantly improving mechanical properties and antibacterial properties of the alloy, solving a bottleneck problem of difficulties in achieving both mechanical properties and biological functions in traditional alloys, and providing a new-generation alloy solution for implantable medical apparatus and instruments.

## Claims

### Claim 1

A high-strength and low-modulus antibacterial alloy, wherein the alloy has a molecular formula of TiaZrbNbcCudAgeOf, wherein subscripts a, b, c, d, e, and f represent atomic percentages of corresponding alloy elements, with 50≤a≤70, 20≤b≤30, 5≤c≤7, 2≤d≤4, 1≤e≤5, 2≤f≤4, and a+b+c+d+e+f=100; and a remainder is an unavoidable impurity.

### Claim 2 (depends on 1)

The high-strength and low-modulus antibacterial alloy according to claim 1, wherein a surface of the high-strength and low-modulus antibacterial alloy is coated with a zinc-strontium three-dimensional network coating.

### Claim 3 (depends on 1)

A method for preparing the high-strength and low-modulus antibacterial alloy according to claim 1, comprising the following steps:
batching: weighing Ti, Zr, Nb, Ag, Cu, and TiO2 according to preset target components of the alloy, and uniformly mixing the same to obtain raw materials for melting, wherein purities of various elements by mass percentage are not lower than 99.0%;
preparation of an alloy ingot using a vacuum arc: placing the raw materials for melting into a vacuum arc device, performing vacuumizing and arc melting in an argon protective atmosphere, and taking out and obtaining the alloy ingot;
preparation of an alloy bar by solidification: placing the alloy ingot into a rapid solidification device, performing vacuumizing and melting in an argon protective atmosphere, and after complete melting, performing spray casting into a copper mold for rapid cooling and solidification within 2-4 min to obtain the alloy bar;
hot working: placing the alloy bar into a heating device, performing vacuumizing, heating up to 950-1,050° C. at 10-20° C./min under rotation in an argon protective atmosphere to ensure uniform heating of the alloy bar, performing heat preservation at such a temperature for 30-60 min, and then taking out the alloy bar for forging and rolling, wherein a deformation amount of the alloy bar is controlled at 10-30% during the process; and
heat treatment: subjecting the hot worked alloy bar to solid solution treatment and aging treatment.

### Claim 4 (depends on 3)

The method for preparing the high-strength and low-modulus antibacterial alloy according to claim 3, wherein during the preparation of the alloy ingot using the vacuum arc, a current is set at 50-120 A, a melting temperature is 1,500-2,500° C., a melting frequency is 4-5 times, and a melting time is 2-3 min each time.

### Claim 5 (depends on 3)

The method for preparing the high-strength and low-modulus antibacterial alloy according to claim 3, wherein the solid solution treatment comprises the following steps: cleaning a surface of the alloy bar to ensure that the surface is free of an impurity and an oxide layer; placing the cleaned alloy bar into a solid solution treatment device, and heating up to 850-950° C. at a heating rate of 30-40° C. per hour in an argon protective atmosphere, wherein the heating rate is not too high to avoid thermal stress caused by a rapid temperature change; performing heat preservation at such a temperature for 2.5-3.5 h, wherein the heat preservation time is not too short to ensure that solute atoms inside the alloy are fully dissolved into a matrix to form a uniform single-phase solid solution; and after the heat preservation is completed, naturally cooling the alloy bar.

### Claim 6 (depends on 5)

The method for preparing the high-strength and low-modulus antibacterial alloy according to claim 5, wherein the aging treatment comprises the following steps: taking the solid solution treated alloy bar out of the solid solution treatment device, and performing surface cleaning; placing the cleaned alloy bar into an aging treatment device, heating up to 500-600° C. at a heating rate of 10-20° C. per hour in an argon protective atmosphere, and performing heat preservation at such a temperature for 3.5-4.5 h, wherein the heat preservation time is not too short to ensure that a precipitate phase is formed inside the alloy to further improve material strength and hardness; and after the heat preservation is completed, naturally cooling the alloy bar.

### Claim 7 (depends on 2)

A method for preparing the high-strength and low-modulus antibacterial alloy according to claim 2, comprising the following steps:
batching: weighing Ti, Zr, Nb, Ag, Cu, and TiO2 according to preset target components of the alloy, and uniformly mixing the same to obtain raw materials for melting, wherein purities of various elements by mass percentage are not lower than 99.0%;
preparation of an alloy ingot using a vacuum arc: placing the raw materials for melting into a vacuum arc device, performing vacuumizing and arc melting in an argon protective atmosphere, and taking out and obtaining the alloy ingot;
preparation of an alloy bar by solidification: placing the alloy ingot into a rapid solidification device, performing vacuumizing and melting in an argon protective atmosphere, and after complete melting, performing spray casting into a copper mold for rapid cooling and solidification within 2-4 min to obtain the alloy bar;
hot working: placing the alloy bar into a heating device, performing vacuumizing, heating up to 950-1,050° C. at 10-20° C./min under rotation in an argon protective atmosphere to ensure uniform heating of the alloy bar, performing heat preservation at such a temperature for 30-60 min, and then taking out the alloy bar for forging and rolling, wherein a deformation amount of the alloy bar is controlled at 10-30% during the process;
heat treatment: subjecting the hot worked alloy bar to solid solution treatment and aging treatment; and
coating with a zinc-strontium three-dimensional network coating: uniformly mixing, in parts by mass, 25-35 parts of a 5-30 wt % calcium silicate solution, 5-9 parts of a 0.5-5.5 wt % zinc nitrate solution, and 5-11 parts of a 0.5-5.5 wt % strontium nitrate solution to form a uniform sol solution, adding 45-65 parts of ethanol to adjust viscosity and uniformity of the sol solution, immersing the high-strength and low-modulus antibacterial alloy in the sol solution for 3-5 min, then slowly lifting the antibacterial alloy to make the sol solution uniformly coated on a surface of the high-strength and low-modulus antibacterial alloy, performing natural air drying, then placing the antibacterial alloy in a heating device for heating to 600-800° C., and performing heat preservation for 1-3 h.

### Claim 8 (depends on 1)

Use of the high-strength and low-modulus antibacterial alloy according to claim 1 in an orthopedic or dental material.

### Claim 9 (depends on 2)

Use of the high-strength and low-modulus antibacterial alloy according to claim 2 in an orthopedic or dental material.

### Claim 10 (depends on 7)

Use of the high-strength and low-modulus antibacterial alloy obtained by the preparation method according to claim 7 in an orthopedic or dental material.