# US 2026/0297704 A1 · Method for antimony recovery and synergistic fluorine fixation from low-grade complex antimony oxide resources

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0297704 A1
- Document ID: US20260297704A1
- Status: Published application
- Kind: A1
- Application number: 19/640,600
- Filed: 2026-04-07
- Published: 2026-10-01
- Earliest claimed: 2025-05-22
- Assignees: Kunming University of Science and Technology
- Applicants: Kunming University of Science and Technology
- Inventors: Hua Wang; Yong Yu; Xiang Liu; Jianhang Hu; Cheng Tan; Luojian Jiwu; Peng Zhu
- Web page: https://patentgrep.com/patent/US20260297704A1

## CPC

- C22B 30/02: Obtaining antimony
- C22B 1/2406: {pelletizing}
- C22B 5/10: by solid carbonaceous reducing agents
- C22B: PRODUCTION AND REFINING OF METALS (electrolytic C25); PRETREATMENT OF RAW MATERIALS

## Abstract

Disclosed is a method for antimony recovery and synergistic fluorine fixation from low-grade complex antimony oxide resources. The disclosure relates to the technical field of efficient recovery and reuse of metal mineral resources. The present disclosure includes (1) crushing low-grade complex antimony oxide resources, mixing with carbonaceous reducing agent A uniformly, and making the mixture I into pellets; (2) drying the pellets obtained in step (1), mixing the dried pellets with carbonaceous reducing agent B, roasting mixture II, collecting the flue gas generated by roasting, and cooling the flue gas to obtain high-quality antimony-containing dust. With the method, efficient and high-quality recovery of antimony from low-grade complex antimony oxide resources through a green and low-cost method is realized, solving the industry's bottleneck problem of efficient utilization of low-grade complex antimony oxide resources.

## Claims

### Claim 1

A method for antimony recovery and synergistic fluorine fixation from low-grade complex antimony oxide resources, comprising following steps:
(1) crushing the low-grade complex antimony oxide resources, mixing with carbonaceous reducing agent A uniformly to obtain mixture I, and then making the mixture I into pellets;
(2) drying the pellets obtained in step (1) to obtain dried pellets, mixing the dried pellets with carbonaceous reducing agent B uniformly to obtain mixture II, roasting the mixture II, collecting flue gas generated by roasting, and cooling the flue gas to obtain high-quality antimony-containing dust;
the low-grade complex antimony oxide resources comprise at least one of senarmontite, valentinite, kermesite, stibiconite, cervantite, sarabauite, romeite, and chemically dissolved antimony, mass fraction of antimony in the low-grade complex antimony oxide resource is 1.0-10%;
a carbon dioxide reactivity of the carbonaceous reducing agent A is higher than that of anthracite in the temperature range of 600-900° C.;
an ash mass fraction of the carbonaceous reducing agent B is less than 18%, and a particle size of the carbonaceous reducing agent B is 74 μm-3 cm.

### Claim 2 (depends on 1)

The method for antimony recovery and synergistic fluorine fixation from low-grade complex antimony oxide resources according to claim 1, wherein in step (1), a particle size of the low-grade complex antimony oxide resources crushed is 50-300 μm.

### Claim 3 (depends on 1)

The method for antimony recovery and synergistic fluorine fixation from low-grade complex antimony oxide resources according to claim 1, wherein the low-grade complex antimony oxide resource further comprises antimony smelting waste, and a mass fraction of the antimony smelting waste in the low-grade complex antimony oxide resource is not more than 15%.

### Claim 4 (depends on 1)

The method for antimony recovery and synergistic fluorine fixation from low-grade complex antimony oxide resources according to claim 1, wherein in step (1), a mass ratio of the low-grade complex antimony oxide resources and the carbonaceous reducing agent A is 100:(1-8).

### Claim 5 (depends on 1)

The method for antimony recovery and synergistic fluorine fixation from low-grade complex antimony oxide resources according to claim 1, wherein in step (2), a roasting heating rate is 5-30° C./min.

### Claim 6 (depends on 1)

The method for antimony recovery and synergistic fluorine fixation from low-grade complex antimony oxide resources according to claim 1, wherein in step (2), a roasting temperature is 600-950° C. and a holding time is 20-220 minutes.

### Claim 7 (depends on 1)

The method for antimony recovery and synergistic fluorine fixation from low-grade complex antimony oxide resources according to claim 1, wherein in step (2), a mass ratio of the pellets and the carbonaceous reducing agent B is 100:(5-30).