# US 2026/0295566 A1 · Catalyst for methane reforming and manufacturing method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0295566 A1
- Document ID: US20260295566A1
- Status: Published application
- Kind: A1
- Application number: 19/478,500
- Filed: 2024-04-02
- Published: 2026-10-01
- Earliest claimed: 2023-04-28
- Assignees: Hanwha Solutions Corporation; Korea Advanced Institute of Science and Technology
- Applicants: Hanwha Solutions Corporation; Korea Advanced Institute of Science and Technology
- Inventors: Junemin BAE; Jeong Hwan CHUN; Yeongmin KIM; Minkee CHOI
- Web page: https://patentgrep.com/patent/US20260295566A1

## CPC

- B01J 23/755: Nickel
- B01J 21/10: Magnesium; Oxides or hydroxides thereof
- B01J 35/615: {100-500 m2/g}
- B01J 35/633: {less than 0.5 ml/g}
- B01J 37/04: Mixing {(B01J37/0009, B01J37/0018 take precedence)}
- B01J 37/10: in the presence of water, e.g. steam
- B01J 37/12: Oxidising
- C07C 1/12: from carbon dioxide with hydrogen
- C07C 9/04: Methane (production by treatment of sewage C02F11/04; natural gas, synthetic natural gas C10L3/06)
- C07C 2523/755: Nickel
- B01J: CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- C07C: ACYCLIC OR CARBOCYCLIC COMPOUNDS

## Abstract

The purpose of the present invention is to provide a nickel catalyst and a manufacturing method thereof, and more specifically, to provide: a structurally stable, highly dispersed nickel catalyst that may be used in methane reforming reaction using carbon dioxide; and a manufacturing method thereof. Provided is a nickel catalyst containing highly dispersed nickel and having excellent structural stability during methane reforming reaction, thus exhibiting excellent catalytic performance in methane reforming reactions using carbon dioxide.

## Claims

### Claim 1

A catalyst for methane reforming comprising aluminum (Al), nickel (Ni), and magnesium (Mg),
and an Al content is 5 mol parts to 50 mol parts based on 100 mol parts of Mg.

### Claim 2 (depends on 1)

The catalyst of claim 1,
wherein the magnesium (Mg) in the catalyst for methane reforming is present in a form of MgO as a support.

### Claim 3 (depends on 1)

The catalyst of claim 1,
wherein a Ni content is 2 parts by weight to 10 parts by weight based on 100 parts by weight of the catalyst for methane reforming.

### Claim 4 (depends on 1)

The catalyst of claim 1,
wherein the catalyst for methane reforming has a BET specific surface area of 100 m2/g to 200 m2/g measured by a nitrogen adsorption method.

### Claim 5 (depends on 1)

The catalyst of claim 1,
wherein the catalyst for methane reforming has a N2 cumulative adsorption pore volume of 0.20 cm3/g to 0.50 cm3/g measured by a nitrogen adsorption method.

### Claim 6 (depends on 1)

The catalyst of claim 1,
wherein the catalyst is used for a methane reforming reaction using carbon dioxide.

### Claim 7

A manufacturing method of a catalyst for methane reforming, comprising:
preparing an aqueous solution mixture by mixing MgO, a nickel (Ni) precursor and aluminum (Al) precursor (step 1);
hydrothermally synthesizing the mixture of step 1 (step 2); and
drying and calcining the hydrothermally synthesized composition of step 2 (step 3);
wherein in step 1, the Al precursor is mixed in an amount such that an Al content is 5 mol parts to 50 mol parts based on 100 mol parts of Mg.

### Claim 8 (depends on 7)

The manufacturing method of claim 7,
wherein in step 1, the Ni precursor is mixed in an amount such that a Ni content is 2 parts of weight to 10 parts of weight based on 100 parts by weight of the catalyst for methane reforming.

### Claim 9 (depends on 7)

The manufacturing method of claim 7,
wherein the aluminum (Al) precursor of step 1 is at least one selected from the group consisting of Al(NO3)3·9H2O, AlCl3·xH2O, Al(OH)3·xH2O, Al2(SO4)3·xH2O, Al2(SO4)3, AlNH4(SO4)2·12H2O, AlCl3·6H2O, AlCl3, AlBr3, AlO4P, AlI3, AlF3, Al(OH)3, Al2(SO4)3, Al2S3, AlN, Al(C5H7O2)3, Al(OC2H5)3, and Al[OCH(CH3)2]3.

### Claim 10 (depends on 7)

The manufacturing method of claim 7,
wherein the nickel (Ni) precursor of step 1 is at least one selected from the group consisting of Ni(CH3COO)2·4H2O), NiCl2, NiCl2·6H2O, Ni(NO3)2, NiSO4, (NH4)2Ni(SO4)2·6H2O, NiBr2, NiCO3, NiF2, NiI2, NiC2O4·2H2O and Ni(ClO4)2·6H2O.

### Claim 11 (depends on 7)

The method of claim 7,
wherein the hydrothermal synthesis of step 2 is performed at a temperature of 100° C. to 300° C. for 12 hours to 48 hours.

### Claim 12 (depends on 7)

The manufacturing method of claim 7,
wherein the drying of step 3 is performed at 50° C. to 150° C. for 2 hours to 24 hours.

### Claim 13 (depends on 7)

The manufacturing method of claim 7,
wherein the calcining of step 3 is performed at 600° C. to 1000° C. for 2 hours to 6 hours.