# US 2026/0285768 A1 · Low-oxygen vanadium aluminum carbide max and manufacturing method therefor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0285768 A1
- Document ID: US20260285768A1
- Status: Published application
- Kind: A1
- Application number: 19/479,897
- Filed: 2024-06-12
- Published: 2026-09-24
- Earliest claimed: 2023-06-13
- Assignees: Korea Institute of Geoscience and Mineral Resources
- Applicants: Korea Institute Of Geoscience And Mineral Resources
- Inventors: Tae-Jun PARK; Sun-Kyung KIM; Ki-Min ROH; Han-Jung KWON
- Web page: https://patentgrep.com/patent/US20260285768A1

## CPC

- C04B 35/5607: {based on refractory metal carbides}
- B01J 27/22: Carbides
- C01B 32/907: Oxycarbides; Sulfocarbides; Mixture of carbides
- C04B 35/6261: {Milling}
- C04B 35/62675: {characterised by the treatment temperature}
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2004/62: Submicrometer sized, i.e. from 0.1-1 micrometer
- C01P 2004/64: Nanometer sized, i.e. from 1-100 nanometer
- C01P 2006/80: Compositional purity
- C04B 2235/3217: Aluminum oxide or oxide forming salts thereof, e.g. bauxite, alpha-alumina
- C04B 2235/3218: Aluminium (oxy)hydroxides, e.g. boehmite, gibbsite, alumina sol
- C04B 2235/3239: Vanadium oxides, vanadates or oxide forming salts thereof, e.g. magnesium vanadate
- C04B 2235/422: Carbon
- C04B 2235/424: Carbon black
- C04B 2235/425: Graphite
- C04B 2235/427: Diamond
- C04B 2235/444: Halide containing anions, e.g. bromide, iodate, chlorite
- C04B 2235/5436: micrometer sized, i.e. from 1 to 100 micron
- C04B 2235/5445: submicron sized, i.e. from 0,1 to 1 micron
- C04B 2235/5454: nanometer sized, i.e. below 100 nm
- C04B 2235/652: Reduction treatment (C04B2235/664 takes precedence)
- C04B 2235/6567: Treatment time
- C04B 2235/658: Atmosphere during thermal treatment
- C04B 2235/6582: Hydrogen containing atmosphere
- C04B 2235/723: Oxygen content
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- B01J: CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS

## Abstract

The present invention provides low-oxygen vanadium aluminum carbide (V2AlC) MAX for producing high-purity vanadium MXene, and a manufacturing method therefor.

## Claims

### Claim 1

A low-oxygen vanadium aluminum carbide MAX, comprising:
vanadium;
aluminum; and
carbon,
wherein the low-oxygen vanadium aluminum carbide MAX is formed by using both an inert gas and hydrogen gas in a carbothermal reaction of the vanadium and the aluminum,
wherein the low-oxygen content ranges from 10 pom to 8.000 ppm, and
wherein a volume ratio of the inert gas to the hydrogen gas ranges from 10:1 to 1:10.

### Claim 2 (depends on 1)

The low-oxygen vanadium aluminum carbide MAX of claim 1,
wherein the low-oxygen vanadium aluminum carbide MAX is formed by:
mixing vanadium oxide, an aluminum compound, and a carbon compound to prepare a mixed powder;
subjecting the mixed powder to a sintering heat treatment to prepare a bulk MAX having a large particle size;
comminuting the bulk MAX to prepare a fine powder MAX; and
subjecting the fine powder MAX to a carbothermal reaction heat treatment using both an inert gas and hydrogen gas such that the low-oxygen vanadium aluminum carbide MAX is formed with reduced oxygen content,
wherein a particle size of the bulk MAX ranges from 50 nm to 100 μm, and
wherein a particle size of the fine powder MAX ranges from 2 mm to 20 μm.

### Claim 3

(canceled)

### Claim 4 (depends on 1)

The low-oxygen vanadium aluminum carbide MAX of claim 1,
wherein the low-oxygen vanadium aluminum carbide MAX has a chemical formula of V2AlC.

### Claim 5 (depends on 2)

The low-oxygen vanadium aluminum carbide MAX of claim 2,
wherein a molar ratio (B/A) of the aluminum compound (B) to the vanadium oxide (A) ranges from 0.2 to 10, and
wherein a molar ratio (C/A) of the carbon compound (C) to the vanadium oxide (A) ranges from 0.2 to 10.

### Claim 6 (depends on 2)

The low-oxygen vanadium aluminum carbide MAX of claim 2,
wherein a particle size of the mixed powder of the vanadium oxide, the aluminum compound, and the carbon compound ranges from 2 nm to 50 μm.

### Claim 7 (depends on 2)

The low-oxygen vanadium aluminum carbide MAX of claim 2,
wherein the vanadium oxide is at least one selected from the group consisting of vanadium pentoxide (V2O5), sodium metavanadate (NaVO3), vanadium trioxide (V2O3), vanadium oxychloride (VOCl3), and ammonium metavanadate (H4NVO3).

### Claim 8 (depends on 2)

The low-oxygen vanadium aluminum carbide MAX of claim 2,
wherein the aluminum compound is at least one selected from the group consisting of alumina (Al2O3), aluminum hydroxide (Al(OH)3), aluminum chloride (AlCl3), aluminum fluoride (AlF3), and aluminum sulfate (Al2(SO4)3).

### Claim 9 (depends on 2)

The low-oxygen vanadium aluminum carbide MAX of claim 2,
wherein the carbon compound is at least one selected from the group consisting of industrial carbon powder, coke, coal, coal tar, activated carbon, natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal

### Claim 10

(canceled)

### Claim 11 (depends on 2)

The low-oxygen vanadium aluminum carbide MAX of claim 2,
wherein a temperature of the sintering heat treatment ranges from 800° C. to 1600° C., and
wherein a time for the sintering heat treatment ranges from 10 minutes to 24 hours.

### Claim 12

(canceled)

### Claim 13

A method for manufacturing a low-oxygen vanadium aluminum carbide MAX, comprising the steps of:
(a-1) preparing a mixed powder by mixing vanadium oxide, an aluminum compound, and a carbon compound;
(a-2) preparing a bulk MAX by subjecting the mixed powder to a sintering heat treatment;
(a-3) preparing a fine powder MAX by comminuting the bulk MAX; and
(a-4) preparing a low-oxygen vanadium aluminum carbide MAX with reduced oxygen content by subjecting the fine powder MAX to a carbothermal reaction heat treatment using both an inert gas and hydrogen gas under an atmosphere of air, vacuum, nitrogen, or argon in a high-temperature synthesis furnace or a super kantal furnace,
wherein a volume ratio of the inert gas to the hydrogen gas ranges from 10:1 to 1:10,
wherein the low-oxygen content ranges from 10 ppm to 8,000 ppm,
wherein a particle size of the bulk MAX ranges from 50 nm to 100 μm, and
wherein a particle size of the fine powder MAX ranges from 2 nm to 20 μm.

### Claim 14 (depends on 13)

The method for manufacturing a low-oxygen vanadium aluminum carbide MAX of claim 13,
wherein, in step (a-1) of preparing a mixed powder by mixing vanadium oxide, an aluminum compound, and a carbon compound,
a mixing ratio of the vanadium oxide, the aluminum compound, and the carbon compound is 1:0.2-0.7:0.1-0.5 by weight.

### Claim 15 (depends on 13)

The method for manufacturing a low-oxygen vanadium aluminum carbide MAX of claim 13,
wherein, in step (a-2) of preparing a bulk MAX by subjecting the mixed powder to a sintering heat treatment,
a temperature of the sintering heat treatment ranges from 800° C. to 1600° C., and
a time for the sintering heat treatment ranges from 10 minutes to 24 hours.

### Claim 16

(canceled)

### Claim 17 (depends on 13)

The method for manufacturing a low-oxygen vanadium aluminum carbide MAX of claim 13,
wherein, in step (a-4) of preparing a low-oxygen vanadium aluminum carbide MAX with reduced oxygen content by subjecting the fine powder MAX to a carbothermal reaction heat treatment using both an inert gas and hydrogen gas under an atmosphere of air, vacuum, nitrogen, or argon in a high-temperature synthesis furnace or a super kantal furnace,
a temperature of the carbothermal reaction heat treatment using both the inert gas and the hydrogen gas ranges from 500° C. to 1100° C., and
a time for the carbothermal reaction heat treatment ranges from 10 minutes to 24 hours.

### Claim 18 (depends on 1)

The use of the low-oxygen vanadium aluminum carbide MAX according to claim 1,
as a MAX phase precursor, a raw material for cemented carbide, a catalyst, or a semiconductor material.

### Claim 19 (depends on 13)

The low-oxygen vanadium aluminum carbide MAX manufactured by the method for manufacturing a low-oxygen vanadium aluminum carbide MAX according to claim 13,
wherein an oxygen content of the low-oxygen vanadium aluminum carbide MAX ranges from 10 ppm to 8,000 ppm.

### Claim 20 (depends on 13)

The use of the low-oxygen vanadium aluminum carbide MAX manufactured by the method for manufacturing a low-oxygen vanadium aluminum carbide MAX according to claim 13,
as a MAX phase precursor, a raw material for cemented carbide, a catalyst, or a semiconductor material.