# US 2026/0275466 A1 · High-strength and low-iron-loss non-oriented electrical steel plate and manufacturing method therefor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0275466 A1
- Document ID: US20260275466A1
- Status: Published application
- Kind: A1
- Application number: 19/162,627
- Filed: 2024-03-06
- Published: 2026-09-17
- Earliest claimed: 2023-03-16
- Assignees: Baoshan Iron & Steel Co., Ltd.
- Applicants: Baoshan Iron & Steel Co., Ltd.
- Inventors: Feng Zhang; Xuejun Lv; Bo Wang; Guobao Li
- Web page: https://patentgrep.com/patent/US20260275466A1

## CPC

- C22C 38/02: containing silicon
- C21D 1/26: Methods of annealing
- C21D 1/28: Normalising
- C21D 1/30: Stress-relieving
- C21D 1/74: Methods of treatment in inert gas, controlled atmosphere, vacuum or pulverulent material
- C21D 1/76: Adjusting the composition of the atmosphere
- C21D 6/00: Heat treatment of ferrous alloys
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/12: during manufacturing of articles with special electromagnetic properties
- C21D 8/1205: involving particular fabrication steps or treatments of ingots or slabs
- C21D 8/1222: {Hot rolling}
- C21D 8/1233: {Cold rolling}
- C21D 8/1238: {Flattening; Dressing; Flexing}
- C21D 8/1244: characterised by the heat treatment
- C21D 8/1255: {with diffusion of elements, e.g. decarburising, nitriding}
- C21D 8/1261: {following hot rolling}
- C21D 8/1266: {between cold rolling steps}
- C21D 8/1272: {Final recrystallisation annealing}
- C21D 8/1283: {Application of a separating or insulating coating}
- C21D 9/46: for sheet metals
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/008: {containing tin}
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/16: containing copper
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- H01F 1/14775: {in the form of sheets}
- H01F 1/14791: {Fe-Si-Al based alloys, e.g. Sendust}
- C22C 2202/02: Magnetic
- H01F 1/16: in the form of sheets (H01F1/147 takes precedence)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES

## Abstract

Disclosed in the present invention is a non-oriented electrical steel plate. In addition to Fe and inevitable impurities, the non-oriented electrical steel plate further contains the following chemical elements in wt %: 0<C≤0.0035%, Si: 2.00-3.80%, Mn: 0.05-1.00%, Al: 0.10-1.20%, and Cu: 0.05-2.00%. Correspondingly, further disclosed in the present invention is a method for manufacturing the non-oriented electrical steel plate, wherein in a heating step, the heating rate of a casting slab in a temperature range of 940-1030° C. is 4.5-8.4° C./min; and in a leveling step, the leveling reduction rate is controlled to be 0.5-8.0%. By using this technical solution, the present invention achieves both low iron-loss performance and high strength.

## Claims

### Claim 1

A non-oriented electrical steel plate, wherein in addition to Fe and inevitable impurities, the non-oriented electrical steel plate further comprises the following chemical elements in wt %:
0<C≤0.0035%, Si: 2.00-3.80%, Mn: 0.05-1.00%, Al: 0.10-1.20%, and Cu: 0.05-2.00%.

### Claim 2 (depends on 1)

The non-oriented electrical steel plate according to claim 1, wherein the non-oriented electrical steel plate consists of the following chemical elements in wt %:
0<C≤0.0035%, Si: 2.00-3.80%, Mn: 0.05-1.00%, Al: 0.10-1.20%, Cu: 0.05-2.00%, and the balance of Fe and inevitable impurities.

### Claim 3 (depends on 1)

The non-oriented electrical steel plate according to claim 1, wherein the non-oriented electrical steel plate further comprises, in wt %, at least one of Sn and Sb in a total amount of 0.005-0.200%, and/or at least one of Ca, Mg, and REM in a total amount of 0.0003-0.0035%.

### Claim 4 (depends on 1)

The non-oriented electrical steel plate according to claim 1, wherein the inevitable impurities comprises at least one of P, S, and N, and their contents satisfy at least one of the following: P≤0.20%, S≤0.0030%, N≤0.0020%.

### Claim 5 (depends on 1)

The non-oriented electrical steel plate according to claim 1, wherein the content of element Cu is 0.10-1.20%.

### Claim 6 (depends on 1)

The non-oriented electrical steel plate according to claim 1, wherein the thickness of the non-oriented electrical steel plate is ≤0.30 mm.

### Claim 7 (depends on 1)

The non-oriented electrical steel plate according to claim 1, wherein the non-oriented electrical steel plate has a yield strength of ≥500 MPa, and a tensile strength of ≥600 MPa.

### Claim 8 (depends on 1)

The non-oriented electrical steel plate according to claim 1, wherein the non-oriented electrical steel plate has an iron loss P10/400 of ≤12.0 W/kg, and a magnetic induction B50 of ≥1.62 T.

### Claim 9 (depends on 1)

A method for manufacturing the non-oriented electrical steel plate according to claim 1, wherein the method comprises the following steps:
(1) smelting and casting to obtain a casting slab;
(2) hot rolling, including heating, rough rolling, finish rolling, and coiling; wherein, in the heating step, a heating rate of the casting slab in a temperature range of 940-1030° C. is 4.5-8.4° C./min;
(3) normalizing annealing;
(4) cold rolling;
(5) continuous annealing; and
(6) leveling and applying an insulating coating to obtain a white steel plate, wherein a leveling reduction rate is 0.5-8.0%, preferably 1.0-5.0%.

### Claim 10 (depends on 9)

The method according to claim 9, wherein the method further comprises:
(7) the white steel plate obtained in step (6) is subjected to stress-relief annealing to obtain a black steel plate.

### Claim 11 (depends on 9)

The method according to claim 9, wherein step (2) satisfies one or more of the following:
in the heating step, a furnace heating time for the casting slab is 120-360 minutes, and a discharge temperature is 1050-1150° C.;
a rough rolling start temperature is 1030-1130° C.;
a finish rolling end temperature is 650-950° C.;
a coiling temperature is 500-850° C.; and
a thickness of the steel plate obtained in step (2) is 1.2-3.0 mm, preferably 1.2-2.0 mm.

### Claim 12 (depends on 9)

The method according to claim 9, wherein in step (3), a soaking temperature for normalizing annealing is 820-980° C., and a soaking time is 1-10 minutes.

### Claim 13 (depends on 9)

The method according to claim 9, wherein in step (4), a single cold rolling is adopted, or a two-stage cold rolling with intermediate annealing is adopted, wherein a soaking temperature of the intermediate annealing is 720-950° C. and a soaking time is 10-60 seconds.

### Claim 14 (depends on 9)

The method according to claim 9, wherein in step (5), a soaking temperature for continuous annealing is 720-950° C., and a soaking time is 10-60 seconds; and/or, a continuous annealing atmosphere is a hydrogen+nitrogen mixed gas, wherein a hydrogen content is 10-45% by volume.

### Claim 15 (depends on 9)

The method according to claim 9, wherein an iron loss P10/400 of the white steel plate obtained in step (6) is ≤19.2 W/kg; preferably, the white steel plate has a yield strength of ≥500 MPa, a tensile strength of ≥600 MPa, and a magnetic induction of B50≥1.62 T.

### Claim 16 (depends on 10)

The method according to claim 10, wherein an iron loss P10/400 of the black steel plate obtained in step (7) is ≤12.0 W/kg; preferably, the black steel plate has a yield strength of ≥500 MPa, a tensile strength of ≥600 MPa, and a magnetic induction of B50≥1.62 T.

### Claim 17 (depends on 2)

The non-oriented electrical steel plate according to claim 2, wherein the content of element Cu is 0.10-1.20%.

### Claim 18 (depends on 2)

The non-oriented electrical steel plate according to claim 2, wherein the thickness of the non-oriented electrical steel plate is ≤0.30 mm.

### Claim 19 (depends on 2)

The non-oriented electrical steel plate according to claim 2, wherein the non-oriented electrical steel plate has a yield strength of ≥500 MPa, and a tensile strength of ≥600 MPa.