# US 2026/0275197 A1 · Hydrophobic lignin-based in-built fire retardant, its preparation and application in polyurethane foam

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0275197 A1
- Document ID: US20260275197A1
- Status: Published application
- Kind: A1
- Application number: 19/080,973
- Filed: 2025-03-17
- Published: 2026-09-17
- Earliest claimed: 2025-03-17
- Assignees: Nano and Advanced Materials Institute Limited
- Applicants: Nano and Advanced Materials Institute Limited
- Inventors: Su Ping BAO; Xin XING; Lei GAO
- Web page: https://patentgrep.com/patent/US20260275197A1

## CPC

- C09K 21/12: containing phosphorus
- C08J 9/0023: {containing oxygen}
- C08J 9/0038: {containing phosphorus}
- C08J 9/0095: {Mixtures of at least two compounding ingredients belonging to different one-dot groups}
- C08J 9/141: {Hydrocarbons}
- C08J 2203/14: Saturated hydrocarbons, e.g. butane; Unspecified hydrocarbons
- C08J 2205/042: Nanopores, i.e. the average diameter being smaller than 0,1 micrometer
- C08J 2205/052: Closed cells, i.e. more than 50% of the pores are closed
- C08J 2205/10: Rigid foams
- C09K: MATERIALS FOR MISCELLANEOUS APPLICATIONS, NOT PROVIDED FOR ELSEWHERE
- C08J: WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H (working, e.g. shaping, of plastics B29)

## Abstract

The present invention provides a simple fabrication process with (no acid, no solvent, halogen-free) environmental-friendly steps to produce a lignin-based fire retardant (LFR) material with in-built fire-retardant functional groups for polyurethane (PU) foam. It also involves the chemical reaction for activating lignin by grafting nonhalogenated phosphate groups of traditional fire retardant with reactive functional groups and changing the original hydrophilic property of traditional fire retardant to hydrophobic property of the novel LFR. A bio-based PU foam with inbuilt fire retardancy is designed by the application of the LFR. The good fire retardancy of the developed PU foam can be achieved without affecting density or compromising thermal conductivity.

## Claims

### Claim 1

A hydrophobic lignin-based in-built fire retardant, comprising:
a lignin source;
an isocyanate component; and
a phosphorous source,
wherein the lignin source is modified by reacting with the isocyanate component prior to reaction with the phosphorous source, forming a stable cross-linked network, and
wherein the hydrophobic lignin-based in-built fire retardant comprises in-built fire-retardant functional groups chemically bonded to the lignin source and exhibits a hydrophobic surface with a water contact angle greater than 120 degrees.

### Claim 2 (depends on 1)

The hydrophobic lignin-based in-built fire retardant of claim 1, wherein the lignin source comprises lignosulfonic acid sodium salt, lignosulfonic acid calcium salt, or alkali lignin.

### Claim 3 (depends on 1)

The hydrophobic lignin-based in-built fire retardant of claim 1, wherein the isocyanate component comprises polymethylene polyphenyl polyisocyanate, diphenylmethane diisocyanate, or a combination thereof.

### Claim 4 (depends on 1)

The hydrophobic lignin-based in-built fire retardant of claim 1, wherein the phosphorous source comprises 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO).

### Claim 5 (depends on 1)

The hydrophobic lignin-based in-built fire retardant of claim 1, wherein the fire retardant is in powder form, having a homogeneous particle size distribution of less than 0.074 mm.

### Claim 6 (depends on 1)

The hydrophobic lignin-based in-built fire retardant of claim 1, wherein the in-built fire-retardant functional groups contribute to a limiting oxygen index (LOI) of at least 26.4% without varying the foam thermal conductivity when incorporated into the polyurethane foams.

### Claim 7 (depends on 1)

The hydrophobic lignin-based in-built fire retardant of claim 1, wherein the hydrophobic lignin-based in-built fire retardant prevents water absorption, thereby maintaining thermal insulation and fire resistance performance of the hydrophobic lignin-based in-built fire retardant over time.

### Claim 8 (depends on 1)

The hydrophobic lignin-based in-built fire retardant of claim 1, wherein the hydrophobic lignin-based in-built fire retardant is free from the use of acids, solvents, or halogens.

### Claim 9

A method of preparing a hydrophobic lignin-based in-built fire retardant, comprising:
reacting a lignin source with an isocyanate component in a reaction system at a temperature of approximately 90° C. for 30 to 90 minutes under nitrogen gas conditions;
adding a phosphorous source into the reaction system and raising the temperature to approximately 120° C. and stirring for 10 to 20 minutes to form a solid product;
drying the solid product at a temperature greater than 70° C. for 15 hours; and
crushing the solid product into a powder and sieving it to obtain a homogeneous particle size distribution of less than 0.074 mm,
wherein the method is conducted in the absence of acids, solvents, and halogens.

### Claim 10 (depends on 9)

The method of claim 9, wherein the lignin source comprises lignosulfonic acid sodium salt, lignosulfonic acid calcium salt, or alkali lignin; the isocyanate component comprises polyaryl polymethylene isocyanate or diphenyl methane diisocyanate; and the phosphorous source comprises 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO).

### Claim 11 (depends on 9)

The method of claim 9, wherein the lignin source is grafted with isocyanate groups from diphenylmethane diisocyanate and non-halogenated phosphate groups from a traditional fire retardant, incorporating reactive functional groups, thereby converting original hydrophilic properties of the traditional fire retardant into hydrophobic properties.

### Claim 12 (depends on 1)

A polyurethane rigid foam with in-built fire retardancy, wherein the polyurethane rigid foam comprises a formulation of:
10-90 parts of bio-based polyol;
10-90 parts of non bio-based polyol;
3 parts of blowing agent;
2-3 parts of foam stabilizer;
0.5-3 parts of catalyst;
0.1-30 parts of fire retardant fillers;
1-10 parts of hydrophobic lignin-based in-built fire retardant of claim 1; and
130-160 parts of isocyanate component;
wherein the polyurethane rigid foam has enhanced fire resistance, and
wherein the polyurethane rigid foam exhibits a hydrophobic surface with a water contact angle greater than 120 degrees.

### Claim 13 (depends on 12)

The polyurethane rigid foam of claim 12, wherein the bio-based polyol is selected from bio-based polyol derived from cashew nut shell oil comprising FX9001, FX9001LV, and FX9011, or caster polyol; and the non bio-based polyol is selected from polyether polyols comprising polyether 403, polyether 4110, polyether 330N.

### Claim 14 (depends on 12)

The polyurethane rigid foam of claim 12, wherein the catalyst comprises amine catalyst, comprising N,N-dicyclohexylmethylamine or triethylenediamine, and dibutyltin dilaurate.

### Claim 15 (depends on 12)

The polyurethane rigid foam of claim 12, wherein the blowing agent comprises water.

### Claim 16 (depends on 12)

The polyurethane rigid foam of claim 12, wherein the isocyanate component comprises polymethylene polyphenyl polyisocyanate, diphenylmethane diisocyanate, or a combination thereof.

### Claim 17 (depends on 12)

The polyurethane rigid foam of claim 12, wherein the foam stabilizer comprises silicone surfactant, polyether polydimethylsiloxane copolymer, organosilicone copolymer.

### Claim 18 (depends on 12)

The polyurethane rigid foam of claim 12, wherein the fire retardant fillers comprise expanded graphite, and dimethyl methylphosphonate.

### Claim 19 (depends on 12)

The polyurethane rigid foam of claim 12, wherein the polyurethane rigid foam exhibits a limiting oxygen index (LOI) of at least 26.4%.

### Claim 20 (depends on 12)

The polyurethane rigid foam of claim 12, wherein the polyurethane rigid foam exhibits a closed-cell structure with a cell size distribution ranging from 50 to 500 microns.