# US 2026/0269660 A1 · Non-oriented electrical steel sheet, motor core, and methods for producing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0269660 A1
- Document ID: US20260269660A1
- Status: Published application
- Kind: A1
- Application number: 18/847,036
- Filed: 2023-03-15
- Published: 2026-09-10
- Earliest claimed: 2022-03-15
- Assignees: Nippon Steel Corporation
- Applicants: Nippon Steel Corporation
- Inventors: Hiroyoshi YASHIKI; Yoshiaki NATORI; Kazutoshi TAKEDA; Ichiro TANAKA; Hiroki HORI
- Web page: https://patentgrep.com/patent/US20260269660A1

## CPC

- H02K 1/02: characterised by the magnetic material
- C21D 1/26: Methods of annealing
- C21D 1/30: Stress-relieving
- C21D 6/008: {containing Si}
- C21D 8/1261: {following hot rolling}
- C21D 8/1272: {Final recrystallisation annealing}
- C21D 8/1283: {Application of a separating or insulating coating}
- C21D 9/46: for sheet metals
- C21D 9/663: Bell-type furnaces
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- H01F 1/14783: {with insulating coating}
- H01F 1/14791: {Fe-Si-Al based alloys, e.g. Sendust}
- H02K 1/04: characterised by the material used for insulating the magnetic circuit or parts thereof
- H02K 15/02: of stator or rotor bodies
- H02K 15/027: Punching the cores
- H02K 15/0273: Laminating the cores
- H02K 15/0275: Annealing the cores
- H02K 15/121: of cores
- B21D 28/22: Notching the peripheries of circular blanks, e.g. laminations for dynamo-electric machines
- C21D 1/76: Adjusting the composition of the atmosphere
- H02K 2215/00: Specific aspects not provided for in other groups of this subclass relating to methods or apparatus specially adapted for manufacturing, assembling, maintaining or repairing of dynamo-electric machines
- Y02P 10/20: Recycling
- H02K: DYNAMO-ELECTRIC MACHINES (dynamo-electric relays H01H53/00; conversion of DC or AC input power into surge output power {H03K3/53})
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES
- B21D: WORKING OR PROCESSING OF SHEET METAL OR METAL TUBES, RODS OR PROFILES WITHOUT ESSENTIALLY REMOVING MATERIAL; PUNCHING METAL (working or processing of wire B21F)
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

Provided is a non-oriented electrical steel sheet including a base metal having a chemical composition containing, by mass %, C: 0.0050% or less, Si: more than 3.70% and 4.60% or less, Mn: more than 0.20% and 0.50% or less, Al: 0.23-0.75%, P: 0.030% or less, S: 0.0018% or less, N: 0.0040% or less, Sn: 0.005-0.040%, Sb: 0-0.040%, with a balance of Fe and impurities, and satisfying [4.2≤Si+Al+0.5×Mn≤4.9], wherein [N]s, an N content from a surface to 20 μm in depth of the base metal, is 0.0060% or less, an average crystal grain size of the base metal is 10 to 30 μm, an iron loss W10/400 is 20.0 W/kg or less, a saturation magnetic flux density is 1.945 T or more, a tensile strength is 680 MPa or more, and a sheet thickness is 0.10 to 0.30 mm.

## Claims

### Claim 1

A non-oriented electrical steel sheet comprising a base metal having a chemical composition containing, by mass %:
C: 0.0050% or less,
Si: more than 3.70% and 4.60% or less,
Mn: more than 0.20% and 0.50% or less,
Al: 0.23 to 0.75%,
P: 0.030% or less,
S: 0.0018% or less,
N: 0.0040% or less,
Ti: less than 0.0050%,
Nb: less than 0.0050%,
Zr: less than 0.0050%,
V: less than 0.0050%,
Cu: less than 0.200%,
Ni: less than 0.500%,
Sn: 0.005 to 0.040%, and
Sb: 0 to 0.040%,
with a balance of Fe and impurities, and
satisfying the Formula (i) below, wherein:
[N]s, an N content from a surface to 20 μm in depth of the base metal, is 0.0060% or less,
an average crystal grain size of the base metal is 10 to 30 μm,
an iron loss W10/400 is 20.0 W/kg or less,
a saturation magnetic flux density is 1.945 T or more,
a tensile strength is 680 MPa or more, and
a sheet thickness is 0.10 to 0.30 mm:
4.2
≤
Si
+
Al
+
0.5
×
Mn
≤
4.9
(
i
)
where, element symbols in the above Formula (i) represents contents (by mass %) of each element.

### Claim 2 (depends on 1)

The non-oriented electrical steel sheet according to claim 1, wherein the steel sheet comprises an insulation coating on a surface of the base metal.

### Claim 3 (depends on 1)

A method of producing a non-oriented electrical steel sheet described in claim 1,
the method including:
a hot rolling process,
a pickling process,
a batch-type hot-band annealing process performed at a soaking temperature of 650 to 780° C. for a soaking time of 8 to 36 hours,
a cold rolling process to reduce a sheet thickness to 0.10 to 0.30 mm, and
a final annealing process at a soaking temperature of 700 to 830° C. for a soaking time of 1 second to 10 minutes,
wherein the hot rolling process, the pickling process, the hot-band annealing process, the cold rolling process, and the final-annealing process are sequentially performed on a steel ingot having a chemical composition containing, by mass %,
C: 0.0050% or less,
Si: more than 3.70% and 4.60% or less,
Mn: more than 0.20% and 0.50% or less,
Al: 0.23 to 0.75%,
P: 0.030% or less,
S: 0.0018% or less,
N: 0.0040% or less,
Ti: less than 0.0050%,
Nb: less than 0.0050%,
Zr: less than 0.0050%,
V: less than 0.0050%,
Cu: less than 0.200%,
Ni: less than 0.500%,
Sn: 0.005 to 0.040%, and
Sb: 0 to 0.040%,
with a balance of Fe and impurities, and
satisfying the Formula (i) below:
4.2
≤
Si
+
Al
+
0.5
×
Mn
≤
4.9
(
i
)
where, element symbols in the above Formula (i) represents contents (by mass %) of each element.

### Claim 4

A motor core comprising a plurality of laminated non-oriented electrical steel sheets,
wherein the chemical composition of the base metal of the non-oriented electrical steel sheet containing, by mass %,
C: 0.0050% or less,
Si: more than 3.70% and 4.60% or less,
Mn: more than 0.20% and 0.50% or less,
Al: 0.23 to 0.75%,
P: 0.030% or less,
S: 0.0018% or less,
N: 0.0040% or less,
Ti: less than 0.0050%,
Nb: less than 0.0050%,
Zr: less than 0.0050%,
V: less than 0.0050%,
Cu: less than 0.200%,
Ni: less than 0.500%,
Sn: 0.005 to 0.040%, and
Sb: 0 to 0.040%,
with a balance of Fe and impurities, and
satisfying the Formula (i) below, wherein:
[N]s, an N content from a surface to 20 μm in depth of the base metal, is 0.0070% or less,
an average crystal grain size of the base metal is 50 to 120 μm,
a saturation magnetic flux density is 1.945 T or more,
a sheet thickness of the non-oriented electrical steel sheet is 0.10 to 0.30 mm:
4.2
≤
Si
+
Al
+
0.5
×
Mn
≤
4.9
(
i
)
where, element symbols in the above Formula (i) represents contents (by mass %) of each element.

### Claim 5 (depends on 4)

The motor core according to claim 4, wherein the non-oriented electrical steel sheet comprises an insulation coating on a surface of the base metal of the non-oriented electrical steel sheet.

### Claim 6 (depends on 4)

A method for producing a motor core described in claim 4,
the method including:
a hot rolling process,
a pickling process,
a batch type hot-band annealing process performed at a soaking temperature of 650 to 780° C. for a soaking time of 8 to 36 hours,
a cold rolling process to reduce the sheet thickness to 0.10 to 0.30 mm,
a final annealing process at a soaking temperature of 700 to 830° C. for a soaking time of 1 second to 10 minutes,
a punching process,
a stacking process,
a stress relief annealing process at a soaking temperature of 750 to 900° C. for 10 to 180 minutes,
wherein the hot rolling process, the pickling process, the hot-band annealing process, the cold rolling process, the final-annealing process, the punching process, the stacking process, and the stress relief annealing process are sequentially performed on a steel ingot having a chemical composition containing, by mass %,
C: 0.0050% or less,
Si: more than 3.70% and 4.60% or less,
Mn: more than 0.20% and 0.50% or less,
Al: 0.23 to 0.75%,
P: 0.030% or less,
S: 0.0018% or less,
N: 0.0040% or less,
Ti: less than 0.0050%,
Nb: less than 0.0050%,
Zr: less than 0.0050%,
V: less than 0.0050%,
Cu: less than 0.200%,
Ni: less than 0.500%,
Sn: 0.005 to 0.040%, and
Sb: 0 to 0.040%,
with a balance of Fe and impurities, and
satisfying the Formula (i) below:
4.2
≤
Si
+
Al
+
0.5
×
Mn
≤
4.9
(
i
)
where, element symbols in the above Formula (i) represents contents (by mass %) of each element.

### Claim 7 (depends on 2)

A method of producing a non-oriented electrical steel sheet described in claim 2,
the method including:
a hot rolling process,
a pickling process,
a batch-type hot-band annealing process performed at a soaking temperature of 650 to 780° C. for a soaking time of 8 to 36 hours,
a cold rolling process to reduce a sheet thickness to 0.10 to 0.30 mm, and
a final annealing process at a soaking temperature of 700 to 830° C. for a soaking time of 1 second to 10 minutes,
wherein the hot rolling process, the pickling process, the hot-band annealing process, the cold rolling process, and the final-annealing process are sequentially performed on a steel ingot having a chemical composition containing, by mass %,
C: 0.0050% or less,
Si: more than 3.70% and 4.60% or less,
Mn: more than 0.20% and 0.50% or less,
Al: 0.23 to 0.75%,
P: 0.030% or less,
S: 0.0018% or less,
N: 0.0040% or less,
Ti: less than 0.0050%,
Nb: less than 0.0050%,
Zr: less than 0.0050%,
V: less than 0.0050%,
Cu: less than 0.200%,
Ni: less than 0.500%,
Sn: 0.005 to 0.040%, and
Sb: 0 to 0.040%,
with a balance of Fe and impurities, and
satisfying the Formula (i) below:
4.2
≤
Si
+
Al
+
0.5
×
Mn
≤
4.9
(
i
)
where, element symbols in the above Formula (i) represents contents (by mass %) of each element.

### Claim 8 (depends on 5)

A method for producing a motor core described in claim 5,
the method including:
a hot rolling process,
a pickling process,
a batch type hot-band annealing process performed at a soaking temperature of 650 to 780° C. for a soaking time of 8 to 36 hours,
a cold rolling process to reduce the sheet thickness to 0.10 to 0.30 mm,
a final annealing process at a soaking temperature of 700 to 830° C. for a soaking time of 1 second to 10 minutes,
a punching process,
a stacking process,
a stress relief annealing process at a soaking temperature of 750 to 900° C. for 10 to 180 minutes,
wherein the hot rolling process, the pickling process, the hot-band annealing process, the cold rolling process, the final-annealing process, the punching process, the stacking process, and the stress relief annealing process are sequentially performed on a steel ingot having a chemical composition containing, by mass %,
C: 0.0050% or less,
Si: more than 3.70% and 4.60% or less,
Mn: more than 0.20% and 0.50% or less,
Al: 0.23 to 0.75%,
P: 0.030% or less,
S: 0.0018% or less,
N: 0.0040% or less,
Ti: less than 0.0050%,
Nb: less than 0.0050%,
Zr: less than 0.0050%,
V: less than 0.0050%,
Cu: less than 0.200%,
Ni: less than 0.500%,
Sn: 0.005 to 0.040%, and
Sb: 0 to 0.040%,
with a balance of Fe and impurities, and
satisfying the Formula (i) below:
4.2
≤
Si
+
Al
+
0.5
×
Mn
≤
4.9
(
i
)
where, element symbols in the above Formula (i) represents contents (by mass %) of each element.