# US 2026/0265886 A1 · Steel sheet, member, and methods for producing the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0265886 A1
- Document ID: US20260265886A1
- Status: Published application
- Kind: A1
- Application number: 19/166,259
- Filed: 2024-03-14
- Published: 2026-09-10
- Earliest claimed: 2023-03-31
- Assignees: Jfe Steel Corporation
- Applicants: JFE Steel Corporation
- Inventors: Kotomi NOGUCHI; Yoichiro MATSUI; Tadachika CHIBA; Hideyuki KIMURA
- Web page: https://patentgrep.com/patent/US20260265886A1

## CPC

- C22C 38/04: containing manganese
- C23C 2/02: Pretreatment of the material to be coated, e.g. for coating on selected surface areas (C23C2/30 takes precedence)
- B32B 15/013: {one layer being formed of an iron alloy or steel, another layer being formed of a metal other than iron or aluminium}
- C21D 1/25: Hardening, combined with annealing between 300 degrees Celsius and 600 degrees Celsius, i.e. heat refining ("Vergüten")
- C21D 1/26: Methods of annealing
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 9/46: for sheet metals
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/06: containing aluminium
- C22C 38/14: containing titanium or zirconium
- C22C 38/20: with copper
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/28: Thermal after-treatment, e.g. treatment in oil bath
- C23C 2/29: {Cooling or quenching}
- C23C 2/40: Plates; Strips
- C25D 3/22: of zinc
- C25D 7/0614: {Strips or foils}
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/004: Dispersions; Precipitations
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR

## Abstract

A steel sheet, a member, and methods for producing the same, are disclosed. The steel sheet has a chemical composition with specified C, Si, Mn, P, S, sol. Al, and N contents and has a steel microstructure containing, in area fractions, a microstructure composed of at least one of ferrite and bainitic ferrite: 10% or more and 60% or less, a microstructure composed of at least one of tempered martensite and lower bainite: 20% or more and 80% or less, retained austenite: 5% or more, and fresh martensite: 10% or less. The average C concentration in the retained austenite is 0.60 mass % or more. In a region within 100 μm from a steel sheet surface in a thickness direction, a content of Fe element present as carbides in the tempered martensite is 0.20 mass % or less on average.

## Claims

### Claim at position 1

1-10. (canceled)

### Claim 11

A steel sheet comprising:
a chemical composition containing, in mass %,
C: 0.10% or more and 0.30% or less,
Si: 0.5% or more and 2.0% or less,
Mn: 1.5% or more and 3.0% or less,
P: 0.10% or less,
S: 0.020% or less,
sol. Al: 1.00% or less,
N: 0.015% or less, and
the balance being Fe and incidental impurities; and
a steel microstructure containing, in area fractions,
a microstructure composed of at least one of ferrite and bainitic ferrite: 10% or more and 60% or less,
a microstructure composed of at least one of tempered martensite and lower bainite: 20% or more and 80% or less,
retained austenite: 5% or more, and
fresh martensite: 10% or less,
wherein:
an average C concentration in the retained austenite is 0.60 mass % or more, and
in a region within 100 μm from a steel sheet surface in a thickness direction, a content of Fe element present as carbides in the tempered martensite is 0.20 mass % or less on average,
and optionally the steel sheet comprises a zinc coating layer on the steel sheet surface.

### Claim 12 (depends on 11)

The steel sheet according to claim 11, wherein the chemical composition further contains, in mass %, at least one element selected from
Ti: 0.100% or less,
Nb: 0.100% or less,
V: 0.100% or less,
B: 0.0050% or less,
Cr: 1.000% or less,
Cu: 1.000% or less,
Sb: 0.200% or less,
Sn: 0.200% or less,
Ta: 0.100% or less,
Ca: 0.0050% or less,
Mg: 0.0050% or less, and
REM: 0.0050% or less.

### Claim 13 (depends on 11)

A member comprising the steel sheet according to claim 11.

### Claim 14 (depends on 12)

A member comprising the steel sheet according to claim 12.

### Claim 15 (depends on 11)

A method for producing a steel sheet, the method comprising:
hot-rolling and cold-rolling a steel slab having the chemical composition according to claim 11 to obtain a cold rolled sheet;
then subjecting the cold rolled steel sheet to an annealing treatment at an annealing temperature of 750° C. or higher and an Ac3 temperature (C) or lower;
then cooling the cold rolled steel sheet in a range from the annealing temperature to a temperature T1 of 200° C. or higher and (Ms temperature (C)-30° C.) or lower at an average cooling rate CR1 of 3° C./s or more and 100° C./s or less;
heating the cold rolled steel sheet in a temperature range from the temperature T1 to a temperature T2 of 300° C. or higher and 450° C. or lower at an average heating rate of 2° C./s or more;
cooling the cold rolled steel sheet in a temperature range from the temperature T2 to a temperature T3 of (T2−150° C.) or higher and (T2−30° C.) or lower at an average cooling rate CR2 of 0.5° C./s or more;
cooling the cold rolled steel sheet in a temperature range from the temperature T3 to a temperature T4 of 150° C. or higher and 350° C. or lower and the temperature T3 or lower at an average cooling rate CR3 of 0.1° C./s or more;
holding the cold rolled steel sheet in a temperature range from 150° C. or higher and 350° C. or lower and the temperature T4 or lower for 20 s or longer and 1000 s or shorter; and
cooling the cold rolled steel sheet to a temperature of 50° C. or lower at an average cooling rate CR4 of 1° C./s or more.

### Claim 16 (depends on 12)

A method for producing a steel sheet, the method comprising:
hot-rolling and cold-rolling a steel slab having the chemical composition according to claim 12 to obtain a cold rolled sheet;
then subjecting the cold rolled steel sheet to an annealing treatment at an annealing temperature of 750° C. or higher and an Ac3 temperature (C) or lower;
then cooling the cold rolled steel sheet in a range from the annealing temperature to a temperature T1 of 200° C. or higher and (Ms temperature (° C.)−30° C.) or lower at an average cooling rate CR1 of 3° C./s or more and 100° C./s or less;
heating the cold rolled steel sheet in a temperature range from the temperature T1 to a temperature T2 of 300° C. or higher and 450° C. or lower at an average heating rate of 2° C./s or more;
cooling the cold rolled steel sheet in a temperature range from the temperature T2 to a temperature T3 of (T2−150° C.) or higher and (T2−30° C.) or lower at an average cooling rate CR2 of 0.5° C./s or more;
cooling the cold rolled steel sheet in a temperature range from the temperature T3 to a temperature T4 of 150° C. or higher and 350° C. or lower and the temperature T3 or lower at an average cooling rate CR3 of 0.1° C./s or more;
holding the cold rolled steel sheet in a temperature range from 150° C. or higher and 350° C. or lower and the temperature T4 or lower for 20 s or longer and 1000 s or shorter; and
cooling the cold rolled steel sheet to a temperature of 50° C. or lower at an average cooling rate CR4 of 1° C./s or more.

### Claim 17 (depends on 11)

A method for producing a steel sheet, the method comprising:
hot-rolling and cold-rolling a steel slab having the chemical composition according to claim 11 to obtain a cold rolled sheet;
then subjecting the cold rolled steel sheet to an annealing treatment at an annealing temperature of 750° C. or higher and an Ac3 temperature (C) or lower;
then cooling the cold rolled steel sheet in a temperature range from the annealing temperature to 500° C. at an average cooling rate CR5 of 5° C./s or more and 100° C./s or less;
retaining the cold rolled steel sheet in a temperature range from 500° C. to a retention stop temperature T5 of an Ms temperature (C) or higher and 320° C. or higher at an average cooling rate CR6 of 10° C./s or less for 10 s or longer and 60 s or shorter;
cooling the cold rolled steel sheet in a temperature range from the retention stop temperature T5 to a temperature T1 of 200° C. or higher and (Ms temperature (° C.)-30° C.) or lower at an average cooling rate CR7 of 3° C./s or more and 100° C./s or less;
heating the cold rolled steel sheet in a temperature range from the temperature T1 to a temperature T2 of 300° C. or higher and 450° C. or lower at an average heating rate of 2° C./s or more;
cooling the cold rolled steel sheet in a temperature range from the temperature T2 to a temperature T3 of (T2−150° C.) or higher and (T2−30° C.) or lower at an average cooling rate CR2 of 0.5° C./s or more;
cooling the cold rolled steel sheet in a temperature range from the temperature T3 to a temperature T4 of 150° C. or higher and 350° C. or lower and the temperature T3 or lower at an average cooling rate CR3 of 0.1° C./s or more;
holding the cold rolled steel sheet in a temperature range from 150° C. or higher and 350° C. or lower and the temperature T4 or lower for 20 s or longer and 1000 s or shorter; and
cooling the cold rolled steel sheet to a temperature of 50° C. or lower at an average cooling rate CR4 of 1° C./s or more.

### Claim 18 (depends on 12)

A method for producing a steel sheet, the method comprising:
hot-rolling and cold-rolling a steel slab having the chemical composition according to claim 12 to obtain a cold rolled sheet;
then subjecting the cold rolled steel sheet to an annealing treatment at an annealing temperature of 750° C. or higher and an Ac3 temperature (C) or lower;
then cooling the cold rolled steel sheet in a temperature range from the annealing temperature to 500° C. at an average cooling rate CR5 of 5° C./s or more and 100° C./s or less;
retaining the cold rolled steel sheet in a temperature range from 500° C. to a retention stop temperature T5 of an Ms temperature (C) or higher and 320° C. or higher at an average cooling rate CR6 of 10° C./s or less for 10 s or longer and 60 s or shorter;
cooling the cold rolled steel sheet in a temperature range from the retention stop temperature T5 to a temperature T1 of 200° C. or higher and (Ms temperature (° C.)-30° C.) or lower at an average cooling rate CR7 of 3° C./s or more and 100° C./s or less;
heating the cold rolled steel sheet in a temperature range from the temperature T1 to a temperature T2 of 300° C. or higher and 450° C. or lower at an average heating rate of 2° C./s or more;
cooling the cold rolled steel sheet in a temperature range from the temperature T2 to a temperature T3 of (T2−150° C.) or higher and (T2−30° C.) or lower at an average cooling rate CR2 of 0.5° C./s or more;
cooling the cold rolled steel sheet in a temperature range from the temperature T3 to a temperature T4 of 150° C. or higher and 350° C. or lower and the temperature T3 or lower at an average cooling rate CR3 of 0.1° C./s or more;
holding the cold rolled steel sheet in a temperature range from 150° C. or higher and 350° C. or lower and the temperature T4 or lower for 20 s or longer and 1000 s or shorter; and
cooling the cold rolled steel sheet to a temperature of 50° C. or lower at an average cooling rate CR4 of 1° C./s or more.

### Claim 19 (depends on 15)

The method for producing a steel sheet according to claim 15, further comprising hot-dip-galvanizing or hot-dip-galvannealing the steel sheet after the steel sheet is cooled at the average cooling rate CR1 of 3° C./s or more and 100° C./s or less.

### Claim 20 (depends on 16)

The method for producing a steel sheet according to claim 16, further comprising hot-dip-galvanizing or hot-dip-galvannealing the steel sheet after the steel sheet is cooled at the average cooling rate CR1 of 3° C./s or more and 100° C./s or less.

### Claim 21 (depends on 17)

The method for producing a steel sheet according to claim 17, further comprising hot-dip-galvanizing or hot-dip-galvannealing the steel sheet after the steel sheet is cooled at the average cooling rate CR7 of 3° C./s or more and 100° C./s or less.

### Claim 22 (depends on 18)

The method for producing a steel sheet according to claim 18, further comprising hot-dip-galvanizing or hot-dip-galvannealing the steel sheet after the steel sheet is cooled at the average cooling rate CR7 of 3° C./s or more and 100° C./s or less.

### Claim 23 (depends on 15)

The method for producing a steel sheet according to claim 15, further comprising electrogalvanizing the steel sheet after the steel sheet is cooled at the average cooling rate CR4 of 1° C./s or more.

### Claim 24 (depends on 16)

The method for producing a steel sheet according to claim 16, further comprising electrogalvanizing the steel sheet after the steel sheet is cooled at the average cooling rate CR4 of 1° C./s or more.

### Claim 25 (depends on 17)

The method for producing a steel sheet according to claim 17, further comprising electrogalvanizing the steel sheet after the steel sheet is cooled at the average cooling rate CR4 of 1° C./s or more.

### Claim 26 (depends on 18)

The method for producing a steel sheet according to claim 18, further comprising electrogalvanizing the steel sheet after the steel sheet is cooled at the average cooling rate CR4 of 1° C./s or more.

### Claim 27 (depends on 11)

A method for producing a member, the method comprising a step of preparing a member by subjecting the steel sheet according to claim 11 to either or both of a forming process and a joining process.

### Claim 28 (depends on 12)

A method for producing a member, the method comprising a step of preparing a member by subjecting the steel sheet according to claim 12 to either or both of a forming process and a joining process.