# US 2026/0264158 A1 · Welding method for bimetal composite pipes for acidic environment

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0264158 A1
- Document ID: US20260264158A1
- Status: Published application
- Kind: A1
- Application number: 19/433,309
- Filed: 2025-12-26
- Published: 2026-09-10
- Earliest claimed: 2025-03-07
- Assignees: Southwest Petroleum University
- Applicants: Southwest Petroleum University
- Inventors: DEZHI ZENG; JIANCHENG LUO; JIE LI; CHENGXIU YU; RUIKANG KE; GUANGGUANG XIANG; LIN YU; JINGYUAN XU; ZHENGPENG DU
- Web page: https://patentgrep.com/patent/US20260264158A1

## CPC

- B23K 9/0282: {for welding tube sections}
- B23K 26/342: Build-up welding
- B23K 9/048: {on cylindrical surfaces}
- B23K 9/167: and of a non-consumable electrode
- B23K 9/173: and of a consumable electrode
- B23K 9/23: taking account of the properties of the materials to be welded
- B23K 9/235: Preliminary treatment
- B23K 10/027: {Welding for purposes other than joining, e.g. build-up welding}
- B23K 26/144: the fluid stream containing particles, e.g. powder
- B23K 26/34: Laser welding for purposes other than joining
- B23K 26/348: in combination with arc heating, e.g. tungsten inert gas [TIG], metal inert gas [MIG] or plasma welding
- B23K 31/12: relating to investigating the properties, e.g. the weldability, of materials
- B23K 2101/06: Tubes
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM

## Abstract

A welding method for bimetal composite pipes for an acidic environment, includes the following steps: (1) machining of a stepped notch; (2) preparation of cladding powder; (3) cleaning and preheating of the composite pipe; (4) laser cladding surfacing; (5) groove designing and machining; (6) groove cleaning and preheating; (7) adding of an isolation layer to the groove; (8) groove cleaning and fit-up; (9) welding and filing of a base layer; and (10) welding of a base layer cover. The welding of composite pipes of the present disclosure is divided into two parts: pre-welding treatment in the factory and post-welding treatment on the site, where the pre-welding treatment in the factory uses advanced equipment and technique such as laser cladding to perform groove pretreatment.

## Claims

### Claim 1

A welding method for bimetal composite pipes for an acidic environment, comprising the following steps:
(1) machining of a stepped notch
first, preparing a finished bimetal composite pipe formed by hydroforming and cleaning a surface and an end face, and then cutting off a certain range of one side of a pipe end near a liner pipe to form the stepped notch,
wherein the stepped notch has a height a of 2.5~4 mm and a depth b of 8~12 mm, and a wall thickness L2 of the liner pipe<the height a of the notch<a wall thickness (L1+L2) of 25% bimetal composite pipe;
(2) preparation of cladding powder
mixing carbon powder, chromium powder, niobium powder, silicon powder, molybdenum powder, manganese powder, iron powder and nickel powder evenly to obtain surfacing layer powder and isolation layer powder respectively,
wherein the surfacing layer powder and the isolation layer powder, by mass percentage, each comprise 0.01%~0.03% of carbon powder, 21%~22% of chromium powder, 3%~3.5% of niobium powder, 0.01%~0.1% of silicon powder, 8%~10% of molybdenum powder, 0.1%~0.3% of manganese powder, and 1%~5% of iron powder, with a balance being nickel powder; and
the surfacing layer powder and the isolation layer powder have a particle size of 5~50 μm and a sphericity of 0.7~0.9;
(3) cleaning and preheating of the composite pipe
performing cleaning and preheating treatment on the bimetal composite pipe with the stepped notch machined in step (1);
(4) laser cladding surfacing
loading the surfacing layer powder in step (2) into a powder feeder of laser cladding equipment, keeping the composite pipe rotating, cladding the surfacing layer powder in the stepped notch in step (1) by using a synchronous laser cladding process in a cladding direction from an inside to an outside, pausing the laser cladding equipment after a surfacing layer is formed, wherein a roundness deviation range of an inner wall surface of the surfacing layer is 0.5%~1%; and polishing an end face of the surfacing layer so that the end face of the surfacing layer is flush with the end face of the composite pipe;
(5) groove designing and machining
machining a V-shaped groove on the end face of the composite pipe after the surfacing in step (4),
wherein for the V-shaped groove, a blunt edge length c is 3~6 mm, a blunt edge thickness d is 2~2.5 mm, and a single-sided groove angle β is 30°±3°;
(6) groove cleaning and preheating
performing cleaning and preheating treatment on the V-shaped groove of the end face of the composite pipe in step (5);
(7) adding of an isolation layer to the groove
loading the isolation layer powder in step (2) into the powder feeder of the laser cladding equipment, keeping the composite pipe rotating, cladding the isolation layer powder on an inclined surface of the V-shaped groove in step (5) by using the synchronous laser cladding process in the cladding direction from the inside to the outside, and stopping the laser cladding equipment after the isolation layer is formed,
wherein a height of the isolation layer is uniform and consistent, the single-sided groove angle β is maintained at 30°±3°, and a thickness e is 2~5 mm;
(8) groove cleaning and fit-up
performing quality inspecting and a cleaning on grooves of two processed to-be-welded composite pipes to ensure that the grooves and surrounding areas thereof are intact, bright and clean, and then performing groove fit-up;
(9) welding and filing of a base layer
performing base layer welding on a bottom of the groove by using tungsten inert gas welding under inert gas protection to form a base weld layer, then performing fill welding on the base weld layer by using the tungsten inert gas welding to form a first fill layer, a second fill layer and a third fill layer; and
(10) welding of a base layer cover
performing cover welding on the base layer by using shielded metal arc welding to form a cover layer.

### Claim 2 (depends on 1)

The welding method for bimetal composite pipes for an acidic environment according to claim 1, wherein in step (3) and step (6), a temperature for the preheating treatment is 80~250° C.

### Claim 3 (depends on 1)

The welding method for bimetal composite pipes for an acidic environment according to claim 1, wherein in step (4) and step (7), parameters of the synchronous laser cladding process are: laser power of 2000~4500 W, a powder feeding speed of 5~15 g/min, a spot diameter of 0.1~0.5 mm, a scanning speed of 90~450 mm/min, and protective gas of argon.

### Claim 4 (depends on 1)

The welding method for bimetal composite pipes for an acidic environment according to claim 1, wherein in step (8), a gap between groove assemblies is 2~3 mm.

### Claim 5 (depends on 1)

The welding method for bimetal composite pipes for an acidic environment according to claim 1, wherein in step (9), for the base layer welding, a welding current is 90~110 A, and a welding speed is 3~4 cm/min; and
for the fill welding, the welding current is 90~110 A, and the welding speed is 4~6 cm/min.

### Claim 6 (depends on 1)

The welding method for bimetal composite pipes for an acidic environment according to claim 1, wherein in step (10), for the cover welding, a welding current is 50~70 A, and a welding speed is 7~9 cm/min.