# US 2026/0258300 A1 · Process for synthesizing europium-doped strontium magnesium germanate phosphors

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0258300 A1
- Document ID: US20260258300A1
- Status: Published application
- Kind: A1
- Application number: 19/675,597
- Filed: 2026-05-13
- Published: 2026-09-03
- Earliest claimed: 2026-05-13
- Assignees: Princess Nourah Bint Abdulrahman University
- Applicants: Princess Nourah Bint Abdulrahman University
- Inventors: Mohd. SHKIR; Thamraa ALSHAHRANI; S. ALFAIFY; H. NAGABHUSHANA; K. MANJUNATHA; B. R. Radha KRUSHNA; S. C. SHARMA; Sambasivam SANGARAJU
- Web page: https://patentgrep.com/patent/US20260258300A1

## CPC

- C09K 11/7735: {Germanates}
- C01G 17/006: {Compounds containing germanium, with or without oxygen or hydrogen, and containing two or more other elements}
- C09D 1/00: Coating compositions, e.g. paints, varnishes or lacquers, based on inorganic substances
- C09D 5/22: Luminous paints {(luminescent compositions C09K11/00)}
- C09D 7/61: inorganic
- C09D 7/80: Processes for incorporating ingredients
- C09K 11/02: Use of particular materials as binders, particle coatings or suspension media therefor
- C09K 11/025: {non-luminescent particle coatings or suspension media}
- C09K 11/77062: {Silicates}
- C09K 11/7708: {Vanadates; Chromates; Molybdates; Tungstates}
- C09K 11/7734: {Aluminates}
- C09K 11/77342: {Silicates}
- C09K 11/7773: {with alkali or alkaline earth metal}
- C09K 11/7792: {Aluminates}
- H10H 20/034: {of coatings}
- H10H 20/8512: {Wavelength conversion materials}
- C01P 2002/54: one element only
- C01P 2002/72: by d-values or two theta-values, e.g. as X-ray diagram
- C01P 2002/77: by unit-cell parameters, atom positions or structure diagrams
- C01P 2002/82: by IR- or Raman-data
- C01P 2002/84: by UV- or VIS- data
- C01P 2002/85: by XPS, EDX or EDAX data
- C01P 2004/03: obtained by SEM
- C01P 2004/04: obtained by TEM, STEM, STM or AFM
- C01P 2006/60: Optical properties, e.g. expressed in CIELAB-values
- C09K: MATERIALS FOR MISCELLANEOUS APPLICATIONS, NOT PROVIDED FOR ELSEWHERE
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C09D: COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR (cosmetics A61K; processes for applying liquids or other fluent materials to surfaces, in general, B05D; staining wood B27K5/02; glazes or vitreous enamels C03C; natural resins, French polish, drying-oils, driers, turpentine, per se, C09F; polishing compositions other than French polish, ski waxes C09G; adhesives or use of materials as adhesives C09J; materials for sealing or packing joints or covers C09K3/10; materials for stopping leaks C09K3/12; processes for the electrolytic or electrophoretic production of coatings C25D)
- H10H: INORGANIC LIGHT-EMITTING SEMICONDUCTOR DEVICES HAVING POTENTIAL BARRIERS
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS

## Abstract

The present invention relates to the synthesis of europium-doped strontium magnesium germanate phosphors and, in more particular manner, to a process for the synthesis of Sr2MgGe2O7:xEu3+ (SMGO:xEu3+) phosphors (where x=0.5-6 mol %) for white LEDs, latent fingerprint detection, and anti-counterfeiting applications. The synthesis is carried out by mixing Stoichiometric molar amounts of strontium nitrate (Sr(NO3)2), magnesium nitrate (Mg(NO3)2·6H2O), germanium dioxide (GeO2), and europium nitrate (Eu(NO3)3·6H2O) were dissolved in deionized water, and further adding Aloe vera gel extract as a natural fuel, wherein the resultant solution is stirred to obtain a homogeneous redox mixture, which then boiled, ignited to form a gel, and combusted into a fine powder, wherein the fine powder is then annealed for improve crystallinity. These results substantiate the efficacy of SMGO:Eu3+ phosphor as a viable forensic material for high-resolution LFP detection, offering a compelling alternative to existing commercial powders, especially under UV-assisted visualization scenarios

## Claims

### Claim 1

A process for synthesizing europium-doped Sr2MgGe2O7 phosphors, the process comprising:
preparing an aloe vera (A.V.) gel extract upon treating fresh aloe vera stems;
(b) dissolving Sr(NO3)2, Mg(NO3)2, Ge(NO3)4, and Eu(NO3)3 corresponding to Eu3+ doping levels of 0-6 mol % in distilled water to form a homogenous solution;
adding Aloe Vera (A.V.) gel extract as both fuel and templating agent to the solution;
stirring the mixture at room temperature for 30 minutes using a magnetic stirrer to form a viscous gel-like solution;
transferring the viscous gel-like solution in a borosilicate beaker and heating in a muffle furnace at 500° C. to initiate an exothermic combustion reaction producing a porous spongy mass;
calcining the porous spongy mass at 800° C. for 4 hours; and
cooling the material at room temperature and collecting thereby grinding using an agate mortar and pestle to obtain the europium-doped Sr2MgGe2O7 (SMGO:x % Eu3+ (x=0-6 mol %)) phosphors, wherein the SrMgGeO4:x % Eu3+ (x=0-6 mol %) phosphors is prepared via a green solution combustion technique, repeated for each Eu3+ concentration from 0 to 6 mol %;
wherein preparing the Sr2MgGe2O7:x % Eu3+ phosphors via the green solution combustion technique comprises preparing a separate precursor batch for each europium concentration by dissolving individually weighed quantities of the metal nitrates in preheated distilled water, adjusting the total oxidizer content by calculating oxygen equivalence from the nitrate ions, adding a measured amount of Aloe vera gel to each batch to establish a fuel-to-oxidizer ratio suitable for self-propagating combustion, stirring each batch until a uniform viscous gel is obtained, and transferring each viscous gel to a designated combustion vessel so that each europium concentration undergoes an independent combustion cycle, and wherein the green solution combustion technique for each europium concentration further comprises heating each viscous gel in a furnace that has been stabilized at a pre-dehydration temperature between 250° C. and 300° C. to remove entrapped moisture, subsequently elevating the furnace temperature to 500° C. to initiate auto-ignition of the gel matrix, permitting the combustion to propagate across the full gel mass through internally generated gases, holding each batch inside the furnace for a settling period after flame extinction to allow post-combustion intermediate phases to consolidate, and collecting the porous spongy mass corresponding to each europium concentration in a separately labeled container, and
wherein the green solution combustion technique for each europium concentration additionally comprises crushing the porous spongy mass obtained from each combustion run, pre-drying each crushed mass at 120-150° C. to eliminate residual volatiles, loading each dried mass into a separate ceramic crucible, calcining each crucible at 800° C. for four hours while maintaining a controlled temperature ramp of 3-5° C. per minute, cooling each crucible naturally to room temperature inside the furnace chamber without forced convection, and subsequently grinding, sieving, and desiccating each calcined phosphor batch independently so that no cross-contamination occurs between different europium doping levels.

### Claim 2 (depends on 1)

The process of claim 1, wherein the preparing of the aloe vera (A.V.) gel extract comprising:
cleaning the fresh Aloe Vera stems thoroughly using distilled water to eliminate surface impurities;
removing an outer green skin from the stems using a sterilized knife and extracting the inner transparent gel;
blending the extracted inner transparent gel to form a smooth and uniform consistency using a household blender; and
storing the prepared A.V. gel extract in a sanitized container for subsequent use.

### Claim 3 (depends on 1)

The process of claim 1, further comprising preparing a first aqueous solution by heating distilled water to 75-85° C. and dissolving strontium nitrate and magnesium nitrate therein until the salts are visually dissolved; preparing a second solution by reacting germanium dioxide with nitric acid until a clear Ge-containing nitrate solution is obtained and filtering the Ge-containing solution through a 0.45 μm PTFE membrane to remove undissolved particulates; combining the first and second solutions and stirring the combined solution at 600-800 rpm until a homogeneous cationic precursor solution is formed; cooling the homogeneous precursor solution to ambient temperature; adding europium nitrate to the cooled precursor solution and stirring until the europium salt is fully dispersed; and thereafter adding the prepared Aloe vera gel extract to the combined nitrate solution while maintaining continuous stirring to give a uniformly mixed precursor gel.

### Claim 4 (depends on 1)

The process of claim 1, further comprising warming the Aloe vera gel extract to 40-50° C. to reduce its viscosity prior to incorporation into the precursor solution; calculating and setting a fuel-to-oxidizer stoichiometry based on the total nitrate oxygen content so that the overall mixture is slightly fuel-lean; adding the warmed Aloe vera gel extract to the homogeneous nitrate solution in a controlled, continuous feed so as to avoid local hot spots; maintaining the mixed system under a controlled shear provided by stirring at 400-550 rpm until the mixture attains a viscous gel state indicative of metal-phytochemical chelation; and holding the resultant viscous gel under gentle agitation for a further 20-40 minutes to permit equilibration of metal-ligand complexes within the gel matrix.

### Claim 5 (depends on 2)

The process of claim 2, further comprising:
mixing synthesized SMGO:2% Eu3+ red-emitting phosphor with blue-emitting BaMgAl10O17:Eu2+ phosphor and a green-emitting (Ba,Sr)2SiO4:Eu2+ phosphor to form a phosphor blend;
combining the phosphor blend with a 398 nm blue LED chip;
mixing the phosphor blend and chip with organic silica gel in a mass ratio of 1:1:2;
stirring the phosphor-silica mixture to ensure even dispersion;
uniformly applying the mixture over the blue LED chip surface; and
curing the composite at 100° C. for 10 hours.

### Claim 6 (depends on 2)

The process of claim 2, further comprising:
mixing 10 mL of distilled water with polyvinyl alcohol (PVA) as a binder;
heating the mixture to 85° C. with continuous stirring to form a clear, uniform solution;
incorporating SMGO:2% Eu3+ phosphor powder into the solution;
subjecting the mixture to ultrasonic treatment for homogeneous dispersion and to prevent particle agglomeration.

### Claim 7 (depends on 1)

The process of claim 1, further comprising transferring the viscous gel into a borosilicate vessel and preheating a muffle furnace to 250-300° C., inserting the vessel into the furnace and maintaining the preheat temperature for a period sufficient to drive off physically adsorbed water, rapidly raising the furnace temperature to 500° C. to initiate self-propagating exothermic combustion across the gel volume, allowing the combustion to proceed to completion such that gaseous products evolve and a porous spongy mass forms, and removing the spongy mass from the furnace after visible cessation of combustion; and breaking the large agglomerates of the porous spongy combustion product to obtain a free-flowing powder; pre-drying the powder at 120-150° C. for 1-2 hours to remove residual moisture and volatile organics; loading the dried powder into a ceramic crucible and placing the crucible into a calcination furnace; increasing the furnace temperature from ambient at a controlled ramp rate of 3-5° C. per minute to 800° C., holding at 800° C. for 4 hours to enable solid-state diffusion and phase formation, and allowing the furnace to cool naturally to room temperature within the closed furnace chamber before unloading the calcined product.

### Claim 8 (depends on 1)

The process of claim 1, further comprising: grinding the calcined mass in an agate mortar and pestle using a circular grinding motion for 20-30 minutes to provide a uniformly milled phosphor powder; sieving the milled powder through a non-metallic sieve having nominal pore dimensions between 100 μm and 150 μm to remove oversized agglomerates; placing the sieved powder into a desiccator to equilibrate under low humidity conditions prior to packaging; and storing the equilibrated powder in sealed, inert-lined containers to prevent atmospheric contamination; and preparing separate precursor batches for each desired europium doping concentration in the range 0-6 mol % by weighing Sr(NO3)2, Mg(NO3)2, Ge precursor and Eu(NO3)3 on an analytical balance to the required molar ratios, dissolving and combining the precursors to form an individual homogeneous solution for each doping level, adding Aloe vera gel to each batch to form a respective viscous gel, subjecting each batch independently to the combustion and calcination sequence.

### Claim 9 (depends on 1)

The process of claim 1, further comprising converting GeO2 to a soluble Ge nitrate prior to precursor mixing by adding a stoichiometric excess of nitric acid, heating the GeO2-acid mixture until complete dissolution of GeO2 is evidenced by the absence of solids, neutralizing any excess acid to a pH of about 3.0-4.0 to maintain ionic activity suitable for metal complexation, filtering the resultant Ge nitrate solution to remove insoluble residues, and immediately using the filtrate in precursor preparation to avoid hydrolytic precipitation; and adjusting the pH of the viscous precursor gel to a value between 3.0 and 4.0 by controlled addition of nitric acid to stabilize dissolved Ge and Eu species, continuing gentle stirring of the pH-adjusted gel for a period of 20-30 minutes to enable redistribution of cations within the Aloe-based chelating matrix, monitoring the viscosity of the gel using a viscometric sensor until the viscosity range of 2-6 Pa s is attained, and transferring the gel to a borosilicate reaction vessel only after said viscosity range is reached.

### Claim 10 (depends on 1)

The process of claim 1, further comprising degassing the homogeneous precursor solution by applying low-pressure evacuation for 3-5 minutes to remove dissolved air pockets that may disrupt combustion, returning the degassed solution to atmospheric pressure, reheating the solution to 40-50° C. to maintain reduced viscosity, and subsequently adding the Aloe vera gel under continuous stirring to form a uniformly aeration-free viscous gel.

### Claim 11 (depends on 1)

The process of claim 1, further comprising:
placing the borosilicate vessel containing the viscous gel in a preheated muffle furnace maintained at 250-300° C. for a pre-dehydration phase, holding the gel at this temperature until steam evolution visibly subsides, raising the temperature rapidly to 500° C. to initiate combustion, and retaining the vessel in the furnace until the combustion front propagates throughout the entire gel matrix and visibly forms a lightweight porous mass; and
allowing the combusted porous mass to remain within the furnace chamber for an additional residence period of 5-10 minutes after flame extinction to stabilize intermediate oxide species, removing the vessel from the furnace while maintaining ambient airflow around the vessel, mechanically crushing the mass immediately while still warm to reduce macro-agglomerates, and then transferring the crushed powder into a drying oven.

### Claim 12 (depends on 1)

The process of claim 1, further comprising:
drying the crushed porous product at 120-150° C. for 1-2 hours to remove moisture generated during combustion, mixing the dried material thoroughly prior to calcination to redistribute fine and coarse fragments, placing the mixed powder into a high-purity ceramic crucible, and positioning the crucible in the central heating zone of a programmable calcination furnace;
initiating calcination by ramping the furnace temperature at 3-5° C. per minute from ambient temperature to 800° C., maintaining a uniform temperature distribution around the crucible by centering the crucible within the furnace, holding the temperature at 800° C. for 4 hours to enable solid-state diffusion pathways to complete, and subsequently allowing the furnace to cool naturally to room temperature without forced ventilation; and
removing the calcined mass from the furnace only after the temperature reaches below 80° C., transferring the calcined mass to an agate mortar, applying continuous circular grinding force until the powder achieves a visually uniform texture, and performing intermediate mixing during grinding to collapse residual agglomerates.

### Claim 13 (depends on 1)

The process of claim 1, further comprising:
sieving the ground phosphor powder through a non-metallic sieve having a nominal pore dimension of 100-150 μm, collecting the fraction of powder that passes through the sieve as the target product, returning the coarse fraction above the sieve to the mortar for additional grinding, and repeating grinding and sieving cycles until no oversized particles remain;
transferring the sieved phosphor powder to a desiccator containing a moisture-adsorbing medium, holding the powder in the desiccator for a conditioning period sufficient to achieve low-humidity equilibrium, and storing the conditioned powder in sealed containers lined with inert polymer coatings for subsequent handling; and
preparing separate precursor mixtures for each europium concentration in the range 0-6 mol %, dissolving metal nitrates for each mixture individually to avoid cross-contamination, adding Aloe vera gel to each solution separately to produce individual viscous gels, and conducting combustion and calcination for each doping level independently so that each concentration yields its own distinct phosphor batch.

### Claim 14 (depends on 1)

The process of claim 1, further comprising:
preparing the Ge nitrate precursor by adding nitric acid dropwise to the GeO2 under continuous stirring, heating the mixture until the GeO2 visibly dissolves, adjusting the resulting solution to a pH of approximately 3.0-4.0 to stabilize the Ge species, filtering the acidified solution to remove insoluble residues, and immediately incorporating the filtered Ge nitrate into the primary precursor mixture; and
maintaining the homogeneous precursor solution at an elevated temperature between 40-50° C. before Aloe vera gel addition to improve miscibility, stirring the mixture under controlled shear conditions until metal-ligand interactions within the gel matrix are visibly established, and aging the gel for an interval of 10-20 minutes to permit rearrangement of metal ions within the gel structure prior to combustion.

### Claim 15 (depends on 1)

The process of claim 1, further comprising:
loading the viscous precursor gel into a muffle furnace that has been pre-stabilized at temperature to avoid transient thermal gradients, allowing the gel to undergo pre-dehydration until visually consistent evaporation occurs, initiating combustion by raising the furnace temperature to 500° C., and maintaining the vessel in the furnace until the internal combustion propagates uniformly across the entire gel structure; forming the final phosphor powder by performing repeated cycles of grinding, drying, calcination, and sieving until the powder reaches a uniform particle distribution suitable for downstream incorporation into devices, and packaging the final powder in moisture-controlled conditions for subsequent use in light-emitting or forensic applications.

### Claim 16 (depends on 1)

The process of claim 1, comprising:
pre-conditioning the distilled water prior to precursor dissolution by heating the water to 90-95° C. to expel dissolved atmospheric gases, cooling the degassed water to 50-60° C. before metal salt dissolution, and subsequently introducing the metal nitrates into the pre-conditioned water in a staggered manner so that each nitrate salt dissolves under identical solvent conditions;
introducing a pre-heating holding period during calcination in which the furnace temperature is retained at 400-450° C. for 20-30 minutes prior to ramping to 800° C., allowing early-stage oxide intermediates to stabilize, and thereafter increasing the temperature at a controlled ramp rate until the set calcination temperature is reached and maintained for the intended duration; and
implementing a post-calcination thermal conditioning phase in which the calcined powder is reheated to a temperature between 200-250° C. for a duration of 15-25 minutes after natural furnace cooling, agitating the powder between reheating intervals to break thermally weakened agglomerates, and cooling the conditioned powder to ambient temperature prior to grinding.