# US 2026/0257208 A1 · Lanthanum oxycarbonate catalyst and its preparation method and application

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0257208 A1
- Document ID: US20260257208A1
- Status: Published application
- Kind: A1
- Application number: 19/130,193
- Filed: 2022-11-15
- Published: 2026-09-03
- Earliest claimed: 2022-11-15
- Assignees: China Petroleum & Chemical Corporation; Sinopec Beijing Research Institute of Chemical Industry
- Applicants: China Petroleum & Chemical Corporation; Sinopec (Beijing) Research Institute of Chemical Industry Co., Ltd.
- Inventors: Jiehua WU; Wei XUE; Huanru WANG; Dongbing LIU; Xue WANG; Yun SHAO
- Web page: https://patentgrep.com/patent/US20260257208A1

## CPC

- B01J 27/232: Carbonates
- B01J 23/10: of rare earths
- B01J 35/395: {Thickness of the active catalytic layer}
- B01J 35/45: Nanoparticles
- B01J 35/51: Spheres
- B01J 35/613: {10-100 m2/g}
- B01J 35/615: {100-500 m2/g}
- B01J 35/633: {less than 0.5 ml/g}
- B01J 35/635: {0.5-1.0 ml/g}
- B01J 35/647: {2-50 nm}
- B01J 35/651: {50-500 nm}
- B01J 35/70: characterised by their crystalline properties, e.g. semi-crystalline (catalysts comprising carbon B01J21/18; molecular sieves B01J29/00)
- B01J 37/0018: {Addition of a binding agent or of material, later completely removed among others as result of heat treatment, leaching or washing,(e.g. forming of pores; protective layer, desintegrating by heat)}
- B01J 37/009: {Preparation by separation, e.g. by filtration, decantation, screening}
- B01J 37/04: Mixing {(B01J37/0009, B01J37/0018 take precedence)}
- B01J 37/088: {Decomposition of a metal salt}
- C07C 2/84: catalytic
- B01J 27/236: Hydroxy carbonates
- B01J 2235/15: X-ray diffraction
- B01J 2235/30: Scanning electron microscopy; Transmission electron microscopy
- C07C 2527/232: Carbonates
- Y02P 20/52: using catalysts, e.g. selective catalysts
- B01J: CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- C07C: ACYCLIC OR CARBOCYCLIC COMPOUNDS
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A lanthanum oxycarbonate catalyst, a preparation method and an application thereof are provided. The lanthanum oxycarbonate catalyst contains hexagonal phase lanthanum oxycarbonate, monoclinic phase lanthanum oxycarbonate containing a doping element and tetragonal phase lanthanum oxycarbonate containing a doping element. The catalyst is used for methane oxidative coupling reaction.

## Claims

### Claim 1

A lanthanum oxycarbonate catalyst, characterized in that the lanthanum oxycarbonate catalyst comprises the following three crystal phases coexisting in a crystalline state: hexagonal phase lanthanum oxycarbonate, monoclinic phase lanthanum oxycarbonate containing a doping element, and tetragonal phase lanthanum oxycarbonate containing a doping element, wherein the ratio of the molar amount of the hexagonal phase lanthanum oxycarbonate to the total molar amount of the tetragonal phase lanthanum oxycarbonate and the monoclinic phase lanthanum oxycarbonate is 1:0.01-1 and the molar ratio of the tetragonal phase lanthanum oxycarbonate and the monoclinic phase lanthanum oxycarbonate is 1:0.1-10.

### Claim 2 (depends on 1)

The lanthanum oxycarbonate catalyst according to claim 1, wherein the doping element in the monoclinic phase lanthanum oxycarbonate and the tetragonal phase lanthanum oxycarbonate is at least one selected from the group consisting of elements of Groups IIA, VIII, IB, IIB and lanthanide elements other than lanthanum, preferably at least one of Mg, Ca, Sr, Ba, Fe, Zn, Ce and Cd, more preferably at least one of Mg, Ca, Sr and Ba;
and/or, the molar ratio of lanthanum element to the doping element in the lanthanum oxycarbonate catalyst is 1:0.01-0.1, preferably 1:0.01-0.08, and more preferably 1:0.012-0.06.

### Claim 3 (depends on 1)

The lanthanum oxycarbonate catalyst according to claim 1, wherein the ratio of the molar amount of the hexagonal phase lanthanum oxycarbonate to the total molar amount of the tetragonal phase lanthanum oxycarbonate and the monoclinic phase lanthanum oxycarbonate is 1:0.1-1, more preferably 1:0.25-0.9; and/or
the molar ratio of the tetragonal phase lanthanum oxycarbonate and the monoclinic phase lanthanum oxycarbonate is 1:0.2-5, preferably 1:0.25-3.

### Claim 4 (depends on 1)

The lanthanum oxycarbonate catalyst according to claim 1, wherein the lanthanum oxycarbonate catalyst has a nanostructure, preferably the catalyst is in a rod form with a hydraulic diameter of 10 nm-40 nm, preferably 10 nm-30 nm, preferably 15 nm-30 nm; or preferably the catalyst is in a flake form with a thickness of 100 nm-500 nm, preferably 200 nm-400 nm; or preferably the catalyst is in a spherical form with a hydraulic diameter of 100 nm-800 nm, preferably 200 nm-600 nm.

### Claim 5 (depends on 1)

The lanthanum oxycarbonate catalyst according to claim 1, wherein the lanthanum oxycarbonate catalyst has a specific surface area of 40 m2/g-100 m2/g, a pore volume of 0.2 cm3/g-0.7 cm3/g, and an average pore size of 5 nm-300 nm, preferably 8 nm-290 nm, and more preferably 180 nm-260 nm.

### Claim 6 (depends on 1)

The lanthanum oxycarbonate catalyst according to claim 1, wherein the lanthanum oxycarbonate catalyst has a rod-shaped nanostructure, a diameter of 10 nm-30 nm, and an aspect ratio of 5-30:1, preferably 10-26:1.

### Claim 7 (depends on 1)

A method for preparing the lanthanum oxycarbonate catalyst as claimed in claim 1, characterized in that the method comprises: adding an alkali solution to a mixed solution containing a lanthanum source and a compound containing a doping element to make the pH value of the mixed system greater than 9, and then sequentially performing reaction, solid-liquid separation, drying and calcination;
wherein, relative to each kilogram of the mixed solution, the addition rate of the alkali solution is 0.01 g/min-10 g/min, preferably 0.03 g/min-8 g/min, and more preferably 0.5 g/min-6 g/min, based on the alkali in the alkali solution; and wherein, firstly, the alkali solution is added dropwise to the mixed solution at a first addition rate until the pH value of the solution reaches a set value, which is between 8 and 9, and then the alkali solution is added dropwise to the mixed solution at a second addition rate until the pH value of the system is 10-13, wherein the second addition rate is 0.5-4.5 g/min higher than the first addition rate.

### Claim 8 (depends on 7)

The method according to claim 7, wherein the lanthanum source is a water-soluble salt of lanthanum, preferably at least one of lanthanum nitrate, lanthanum chloride and lanthanum acetate, and more preferably lanthanum nitrate.

### Claim 9 (depends on 7)

The method according to claim 7, wherein the concentration of the alkali solution is 2 wt %-25 wt %, preferably 3 wt %-20 wt %, and more preferably 5 wt %-18 wt %.

### Claim 10 (depends on 7)

The method according to claim 7, wherein the alkali in the alkali solution is a compound of a Group IA metal.

### Claim 11 (depends on 7)

The method according to claim 7, wherein the first addition rate is 0.01-1 g/min; and/or the second addition rate is 0.5-5 g/min.

### Claim 12 (depends on 7)

The method according to claim 7, wherein the reaction temperature is 80-200° C. and the reaction time is 10 h-50 h;
and/or, the drying temperature is 60° C.-100° C., and the drying time is 12 h-24 h;
and/or, the calcination temperature is 450° C.-550° C., and the calcination time is 2 h-8 h.

### Claim 13 (depends on 7)

The method according to claim 7, wherein the method further comprises:
S1. under a first stirring condition, mixing the lanthanum source and the compound containing the doping element with water to obtain a mixed solution; preferably, the first stirring condition includes: a temperature of 10-50° C., a rotation speed of 300-1000 rpm, and a time of 10-40 min;
S2. under a second stirring condition, adding the alkali solution to the mixed solution to obtain a mixed system; preferably, the second stirring condition includes: a temperature of 20-60° C. and a rotation speed of 500-1500 rpm.

### Claim 14 (depends on 1)

A lanthanum oxycarbonate catalyst composition, comprising the lanthanum oxycarbonate catalyst according to claim 1 and a binder, wherein the binder comprises alumina, soluble starch, silica sol and polyethylene glycol.

### Claim 15 (depends on 1)

A lanthanum oxycarbonate catalyst composition, comprising the lanthanum oxycarbonate catalyst according to claim 1 and a support, wherein the support comprises alumina, silica, molecular sieve, diatomaceous earth and ceramic.

### Claim 16 (depends on 1)

Use of the lanthanum oxycarbonate catalyst according to claim 1 in the oxidative coupling reaction of methane to produce C2+ hydrocarbons.

### Claim 17 (depends on 1)

A method for preparing C2+ hydrocarbons from methane, characterized in that the method comprises: contacting methane with the lanthanum oxycarbonate catalyst according to claim 1 for reaction in the presence of oxygen and under the conditions of methane oxidative coupling reaction.

### Claim 18 (depends on 17)

The method according to claim 17, wherein the molar ratio of methane to oxygen is 2-9:1;
and/or, the contact and reaction temperature is 450° C.-650° C.;
and/or, the space velocity of methane is 5000 mL/(g·h)-200000 mL/(g·h).