# US 2026/0250204 A1 · High-Entropy Alloy Sulfide/Two-Dimensional Nano Composite Material, Preparation Method Therefor, and Application Thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0250204 A1
- Document ID: US20260250204A1
- Status: Published application
- Kind: A1
- Application number: 18/714,200
- Filed: 2023-04-07
- Published: 2026-08-27
- Earliest claimed: 2022-04-12
- Assignees: C-Star (Guangzhou) Nano Materials Co., Ltd
- Applicants: C-Star (Guangzhou) Nano Materials Co., Ltd
- Inventors: Haihua Shen; Gongchang Zeng; Heping Zeng
- Web page: https://patentgrep.com/patent/US20260250204A1

## CPC

- C04B 35/547: based on sulfides or selenides {or tellurides}
- C04B 35/6264: {Mixing media, e.g. organic solvents}
- C04B 35/62655: {Drying, e.g. freeze-drying, spray-drying, microwave or supercritical drying}
- C04B 35/62675: {characterised by the treatment temperature}
- C04B 2235/3272: Iron oxides or oxide forming salts thereof, e.g. hematite, magnetite
- C04B 2235/3279: Nickel oxides, nickalates, or oxide-forming salts thereof
- C04B 2235/3281: Copper oxides, cuprates or oxide-forming salts thereof, e.g. CuO or Cu2O
- C04B 2235/3284: Zinc oxides, zincates, cadmium oxides, cadmiates, mercury oxides, mercurates or oxide forming salts thereof
- C04B 2235/3843: Titanium carbides
- C04B 2235/3856: Carbonitrides, e.g. titanium carbonitride, zirconium carbonitride
- C04B 2235/425: Graphite
- C04B 2235/446: Sulfides, tellurides or selenides
- C04B 2235/449: Organic acids, e.g. EDTA, citrate, acetate, oxalate
- H05K 9/0081: {Electromagnetic shielding materials, e.g. EMI, RFI shielding (H05K9/0003 takes precedence)}
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- H05K: PRINTED CIRCUITS; CASINGS OR CONSTRUCTIONAL DETAILS OF ELECTRIC APPARATUS; MANUFACTURE OF ASSEMBLAGES OF ELECTRICAL COMPONENTS

## Abstract

The present application discloses a high-entropy alloy sulfide/two-dimensional nano composite material, a preparation method therefor, and an application thereof. According to the present application, zinc acetate, copper acetate, ferric acetate, nickel acetate, and cadmium acetate are dissolved in an organic solvent, then a sulfide and a two-dimensional nano material are added, dispersed, and uniformly mixed for reaction, and the high-entropy alloy sulfide/two-dimensional nano composite material is prepared in situ in one step. According to the present application, tests show that a nano high-entropy alloy sulfide has an electromagnetic wave absorption effect in a wave band of 6-18 GHz, and after the nano high-entropy alloy sulfide is compounded with the two-dimensional nano material, the wave band of the electromagnetic wave absorption effect is expanded to 5-18 GHz, and the electromagnetic wave absorption capability is improved.

## Claims

### Claim 1

A preparation method for a high-entropy alloy sulfide/two-dimensional nano composite material, comprising the following steps:
S1: dissolving zinc acetate, copper acetate, ferric acetate, nickel acetate, and cadmium acetate in an organic solvent, then adding a sulfide and a two-dimensional nano material, dispersing and uniformly mixing to obtain a mixed solution; and
S2: heating the mixed solution obtained in step S1 to 140-220° C. for reaction, cooling to room temperature after heat preservation, performing centrifugal separation at room temperature, and washing and drying the centrifuged product to obtain the high-entropy alloy sulfide/two-dimensional nano composite material, wherein
the zinc acetate, the copper acetate, the ferric acetate, the nickel acetate and the cadmium acetate are added at an equal or approximately equal molar ratio; the sulfide is selected from one of thiourea, aminothiourea and thioacetamide; and the two-dimensional nano material is selected from one of Ti3C2 MXene, g-C3N4, graphene and their oxides.

### Claim 2 (depends on 1)

The preparation method according to claim 1, wherein in step S1, the organic solvent is one or a combination of more of ethylenediamine, triethanolamine, phenylacetonitrile, and acetonitrile.

### Claim 3 (depends on 1)

The preparation method according to claim 1, wherein in step S1, the content of a two-dimensional nano material in the mixed solution is 1-15%, based on a total weight of the mixed solution.

### Claim 4 (depends on 1)

The preparation method according to claim 1, wherein in step S1, a molar ratio of the zinc acetate, the copper acetate, the ferric acetate, the nickel acetate or the cadmium acetate to the sulfide is 1:(2-5).

### Claim 5 (depends on 1)

The preparation method according to claim 1, wherein in step S2, the heating refers to programmed heating to 140-220° C. at a rate of 1-5° C./min.

### Claim 6 (depends on 1)

The preparation method according to claim 1, wherein in step S2, the heat preservation time is 12-24 h.

### Claim 7 (depends on 1)

The preparation method according to claim 1, wherein in step S2, the washing is carried out with deionized water and/or absolute ethanol.

### Claim 8 (depends on 1)

The preparation method according to claim 1, wherein in step S2, the drying temperature is 80-100° C.

### Claim 9

(canceled)

### Claim 10

(canceled)

### Claim 11 (depends on 1)

A high-entropy alloy sulfide/two-dimensional nano composite material, wherein the high-entropy alloy sulfide/two-dimensional nano composite material is prepared by the preparation method according to claim 1.

### Claim 12 (depends on 2)

A high-entropy alloy sulfide/two-dimensional nano composite material, wherein the high-entropy alloy sulfide/two-dimensional nano composite material is prepared by the preparation method according to claim 2.

### Claim 13 (depends on 3)

A high-entropy alloy sulfide/two-dimensional nano composite material, wherein the high-entropy alloy sulfide/two-dimensional nano composite material is prepared by the preparation method according to claim 3.

### Claim 14 (depends on 4)

A high-entropy alloy sulfide/two-dimensional nano composite material, wherein the high-entropy alloy sulfide/two-dimensional nano composite material is prepared by the preparation method according to claim 4.

### Claim 15 (depends on 5)

A high-entropy alloy sulfide/two-dimensional nano composite material, wherein the high-entropy alloy sulfide/two-dimensional nano composite material is prepared by the preparation method according to claim 5.

### Claim 16 (depends on 6)

A high-entropy alloy sulfide/two-dimensional nano composite material, wherein the high-entropy alloy sulfide/two-dimensional nano composite material is prepared by the preparation method according to claim 6.

### Claim 17 (depends on 7)

A high-entropy alloy sulfide/two-dimensional nano composite material, wherein the high-entropy alloy sulfide/two-dimensional nano composite material is prepared by the preparation method according to claim 7.

### Claim 18 (depends on 8)

A high-entropy alloy sulfide/two-dimensional nano composite material, wherein the high-entropy alloy sulfide/two-dimensional nano composite material is prepared by the preparation method according to claim 8.