# US 2026/0245769 A1 · Electric wire

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0245769 A1
- Document ID: US20260245769A1
- Status: Published application
- Kind: A1
- Application number: 19/162,043
- Filed: 2024-03-08
- Published: 2026-08-20
- Earliest claimed: 2023-03-10
- Assignees: Prime Polymer Co., Ltd.
- Applicants: Prime Polymer Co., Ltd.
- Inventors: Sumiaki FUJII; Yoshio YANAGISHITA
- Web page: https://patentgrep.com/patent/US20260245769A1

## CPC

- H01B 3/441: {from alkenes}
- H01B 3/307: {Other macromolecular compounds}
- H01B 7/0275: {comprising one or more extruded layers of insulation}
- H01B 7/295: using material resistant to flame
- H01B: CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES (selection for magnetic properties H01F1/00; waveguides H01P {; printed circuits H05K})

## Abstract

An electric wire having a coating layer that is excellent in an electric resistance property and mechanical strength and that has a satisfactory appearance is provided by using an insulating material that is excellent in extrusion processability containing a polymer containing ethylene as a main component. The electric wire includes a conductor or a conductor-shielding layer that is coated with the insulating material containing a polymer containing ethylene as a main component, wherein, with regard to the polymer containing ethylene as a main component, a density is in a specific range; a melt flow rate (MFR) is in a specific range; a volume resistivity (Ω·cm) is in a specific range; a shear viscosity (Pa·s) is in a range that forms a specific flow curve; and a 50% failure time (F50) in an environmental stress cracking resistance test (E.S.C.R. test) is in a specific range.

## Claims

### Claim 1

An electric wire comprising a conductor or a conductor-shielding layer that is coated with an insulating material containing a polymer containing ethylene as a main component, wherein the polymer containing ethylene as a main component satisfies the conditions (a) to (e) shown below:
(a) a density as measured in accordance with JIS K 6922 is 900 to 925 kg/m3;
(b) a melt flow rate (MFR) (temperature: 190° C.; load: 21.18 N) as measured in accordance with JIS K 6921 is 10 to 25 g/10 min;
(c) a volume resistivity (2 mm-thick press sheet) as measured in accordance with ASTM D257:2007 is 1.0×1016 Ω·cm or more;
(d) a shear viscosity at a shear rate of 12.2 (1/s) is 300 (Pa·s) or more and 8000 (Pa·s) or less, and a shear viscosity at a shear rate of 2432 (1/s) is 30 (Pa·s) or more and 220 (Pa·s) or less, as measured by using a capillary rheometer,
Method for measurement:
Melt viscosity (flow curve) measurement:
Apparatus: capillary rheometer “CAPILOGRAPH 1D” (Toyo Seiki Seisaku-sho, Ltd.);
Capillary: L=30 mm, D=1 mm, inflow angle=180°;
Piston speed: 1, 2, 5, 10, 20, 50, 100, 200 mm/min; and
Measurement temperature: 190° C.; and
(e) a 50% failure time (F50) at an environmental stress cracking resistance (E.S.C.R. test; 3 mm-thick press sheet;
test temperature: 65° C.) as measured in accordance with ASTM D1693 is 10 hours or more.

### Claim 2 (depends on 1)

The electric wire according to claim 1, wherein (c) the volume resistivity (2 mm-thick press sheet) of the polymer containing ethylene as a main component as measured in accordance with ASTM D257:2007 is 1.0×1016 Ω·cm or more and 1.0×1019 Ω·cm or less.

### Claim 3 (depends on 1)

The electric wire according to claim 1, wherein the polymer containing ethylene as a main component of the insulating material is a copolymer of ethylene and an α-olefin having 3 to 20 carbon atoms.

### Claim 4 (depends on 1)

The electric wire according to claim 1, wherein a flame retardant is compounded in the insulating material.

### Claim 5 (depends on 1)