# US 2026/0234839 A1 · Preparation method of high-temperature-resistant polyacrylonitrile-based carbon fibre and its application in fireproof fabric

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0234839 A1
- Document ID: US20260234839A1
- Status: Published application
- Kind: A1
- Application number: 19/565,588
- Filed: 2026-03-13
- Published: 2026-08-13
- Earliest claimed: 2025-02-12
- Assignees: Zhejiang Taizhou Jingzhen Technology Co., Ltd.; Wuxi Tanyan Technology Co., Ltd.
- Applicants: Zhejiang Taizhou Jingzhen Technology Co., Ltd.; Wuxi Tanyan Technology Co., Ltd.
- Inventors: Bin XING; Bin FANG; Yuanhao WANG; Yewen LUO; Weiyang CHEN
- Web page: https://patentgrep.com/patent/US20260234839A1

## CPC

- D01F 9/22: from polyacrylonitriles
- D01D 5/06: Wet spinning methods {(D01D5/0046 takes precedence)}
- D01F 6/18: from polymers of unsaturated nitriles, e.g. polyacrylonitrile, polyvinylidene cyanide
- D01F 6/38: comprising unsaturated nitriles as the major constituent
- D01F 9/225: {from stabilised polyacrylonitriles}
- D10B 2101/12: Carbon; Pitch
- D10B 2401/04: Heat-responsive characteristics
- D01F: CHEMICAL FEATURES IN THE MANUFACTURE OF ARTIFICIAL FILAMENTS, THREADS, FIBRES, BRISTLES OR RIBBONS; APPARATUS SPECIALLY ADAPTED FOR THE MANUFACTURE OF CARBON FILAMENTS
- D01D: MECHANICAL METHODS OR APPARATUS IN THE MANUFACTURE OF ARTIFICIAL FILAMENTS, THREADS, FIBRES, BRISTLES OR RIBBONS
- D10B: INDEXING SCHEME ASSOCIATED WITH SUBLASSES OF SECTION D, RELATING TO TEXTILES

## Abstract

This invention provides a preparation method for high-temperature-resistant polyacrylonitrile-based carbon fiber for fireproof fabric. By incorporating 2-acrylamido-2-methylpropane sulfonic acid, hydrogen bromide, and basic aluminum chloride, the fiber's fire resistance, flexibility, and limiting oxygen index are enhanced. Pre-oxidation via radiation heating inhibits skin-core structures, while ultrasonic cleaning removes impurities. Treatment with sodium β-anthraquinone sulfonate improves tensile strength, yielding high-strength, fire-resistant carbon fiber.

## Claims

### Claim 1

A preparation method of high-temperature-resistant polyacrylonitrile-based carbon fibre, which is characterized in that it includes the following steps:
Step S1—prepare Spinning Stock A: dissolve polyacrylonitrile based copolymer in dimethylacetamide to make the mass concentration of polyacrylonitrile based copolymer reach 20%~30%, and then prepare Spinning Stock A;
Step S2—add accelerator: add accelerator 2-acrylamido-2-methylpropane sulfonic acid to Spinning Stock A to prepare Spinning Stock B;
Step S3—add polyoxyethylene sorbitan monopalmitate: add polyoxyethylene sorbitan monopalmitate to Spinning Stock B to prepare Spinning Stock C;
Step S4—prepare polyacrylonitrile fibre precursor: take the aqueous solution of dimethylacetamide with mass concentration of 40%~50% as the coagulation bath, use the wet spinning method to spin Spinning Stock C, draw and stretch to prepare polyacrylonitrile fibre precursor I;
Step S5—perform perfluoro lauryl alcohol polyoxyethylene ether treatment: dip polyacrylonitrile fibre precursor I into perfluoro lauryl alcohol polyoxyethylene ether aqueous solution, and then dry to prepare polyacrylonitrile fibre precursor II;
Step S6—spray basic aluminum chloride: spray the basic aluminum chloride aqueous solution on polyacrylonitrile fibre precursor II, and then dry to make polyacrylonitrile fibre precursor III;
Step S7—spray carbon powder: disperse the carbon powder in the aqueous solution of perfluoro lauryl alcohol polyoxyethylene ether of Step S5 to prepare Solution D, spray Solution D on polyacrylonitrile fibre precursor III, and then dry to prepare polyacrylonitrile fibre precursor IV;
Step S8—prepare preoxidation gas atmosphere: replace the gas in the preoxidation chamber with a mixture of oxygen and hydrogen bromide;
Step S9—conduct radiation heating preoxidation: place polyacrylonitrile fibre precursor IV in the gas atmosphere of Step S8, and preoxidize by radiation heating to produce pre-oxidized fibre V;
Step S10—conduct ultrasonication: immerse the pre-oxidized fibre V in the aqueous solution of sodium β-anthraquinone sulfonate, and use ultrasonication to prepare the pre-oxidized fibre VI; wherein an ultrasonic frequency is 100 KHz-200 KHz; an ultrasonic treatment time is 10 min-30 min; a mass concentration of an aqueous solution of sodium beta-anthraquinone sulfonate is 15%-25%;
Step S11—perform perfluoro lauryl alcohol polyoxyethylene ether treatment: dip the pre-oxidized fibre VI in the aqueous solution of perfluoro lauryl alcohol polyoxyethylene ether, and then dry to prepare the pre-oxidized fibre VII;
Step S12—perform carbonization treatment: place the pre-oxidized fibre VII in nitrogen for heating and carbonization to produce polyacrylonitrile-based carbon fibre, wherein a carbonization temperature is 800° C.-1200° C.; a carbonization time is 1 h-2 h.

### Claim 2 (depends on 1)

The preparation method stated in claim 1, which is characterized in that the molar ratio of acrylonitrile monomer and vinyl acetate in the polyacrylonitrile based copolymer is 100:1~100:10.

### Claim 3 (depends on 2)

The preparation method stated in claim 2, which is characterized in that the molar ratio of 2-acrylamido-2-methylpropane sulfonic acid and acrylonitrile monomer is 0.1:100~0.2:100.

### Claim 4 (depends on 3)

The preparation method stated in claim 3, which is characterized in that the mass ratio of the polyoxyethylene sorbitan monopalmitate and polyacrylonitrile based copolymer is 0.2:100~0.4:100.

### Claim 5 (depends on 4)

The preparation method stated in claim 4, which is characterized in that the size of the polyacrylonitrile fibre precursor I is 2D~5D.

### Claim 6 (depends on 5)

The preparation method stated in claim 5, which is characterized in that the mass concentration of the aqueous solution of perfluoro lauryl alcohol polyoxyethylene ether is 1.5%~2.5%; the dipping time is 1 h~2 h; the drying temperature is 110° C.~130° C.

### Claim 7 (depends on 6)

The preparation method stated in claim 6, which is characterized in that the mass concentration of the alkaline aluminum chloride aqueous solution is 1%~2%; the drying temperature is 110° C.~130° C.

### Claim 8 (depends on 7)

The preparation method stated in claim 7, which is characterized in that the mass concentration of the carbon powder in Solution Dis 5%~15%, and the particle size of the carbon powder is 6 μm~10 μm; the drying temperature is 110° C.~130° C.

### Claim 9 (depends on 8)

A high-temperature-resistant polyacrylonitrile-based carbon fibre, which is characterized in that the high-temperature-resistant polyacrylonitrile-based carbon fibre is fabricated with the preparation method stated in claim 8.

### Claim 10 (depends on 9)

The application of high-temperature-resistant polyacrylonitrile-based carbon fibre in fireproof fabric stated in claim 9.