# US 2026/0234005 A1 · Method for dry recycling and structure regeneration of layered carbon materials

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0234005 A1
- Document ID: US20260234005A1
- Status: Published application
- Kind: A1
- Application number: 19/640,429
- Filed: 2026-04-07
- Published: 2026-08-13
- Earliest claimed: 2025-09-29
- Assignees: Rikomay Recycling Singapore Pte. Ltd.
- Applicants: Rikomay Recycling Singapore Pte. Ltd.
- Inventors: Yu ZHANG; Yuancheng CAO; Jianfeng ZHANG; Sheng QIAN; Huxun LUO; Xiaoxi PENG; Tian ZHENG; Hang LIAO; Fan HU; Bin ZHOU
- Web page: https://patentgrep.com/patent/US20260234005A1

## CPC

- C01B 32/05: Preparation or purification of carbon not covered by groups C01B32/15, C01B32/20, C01B32/25, C01B32/30
- C01B 32/205: Preparation
- C01B 32/184: Preparation
- C01B 32/215: Purification; Recovery or purification of graphite formed in iron making, e.g. kish graphite
- H01M 4/583: Carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 10/54: Reclaiming serviceable parts of waste accumulators
- C01P 2002/82: by IR- or Raman-data
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS

## Abstract

A method for dry recycling and structure regeneration of a layered carbon material, in which a waste layered carbon material is pretreated, mixed with asphalt, and subjected to gas-phase infiltration in a nitrogen atmosphere at 300-500° C., pyrolytic deposition at 800° C. under vacuum, and isostatic-pressing densification at 5 MPa in an inert gas atmosphere to obtain an intermediate product; the intermediate product is heated from 800° C. to 1500° C., from 1500° C. to 2500° C., from 2500° C. to 2850° C., kept at 2850° C. under an axial pulse pressure for 1-6 h; and the resultant product is cooled and post-treated.

## Claims

### Claim 1

A method for dry recycling and structure regeneration of layered carbon materials, comprising:
(S10) pretreating a waste layered carbon material;
(S20) mixing a pretreated waste layered carbon material with asphalt, followed by gas-phase infiltration in a nitrogen atmosphere at 300-500° C. to allow small-molecule aromatic hydrocarbons to diffuse into defect sites of the pretreated waste layered carbon material, so as to obtain a mixture;
performing pyrolytic deposition on the mixture at 800° C. under vacuum to obtain a first intermediate product, wherein the small-molecule aromatic hydrocarbons undergo dehydrogenation condensation to release hydrogen gas and form polycyclic aromatic hydrocarbon radicals, and the polycyclic aromatic hydrocarbon radicals undergo in-situ condensation through polymerization at the defect sites of the pretreated waste layered carbon material to form a continuous carbon film; performing isostatic-pressing densification on the first intermediate product at a pressure of 5-7 MPa in an inert gas atmosphere to force the continuous carbon film to experience plastic flow and fill micropores with a size smaller than 50 nm to obtain a second intermediate product;
(S30) heating the second intermediate product from 800° C. to 1500° C. at a rate of 5-10° C./min to realize defect identification and transformation to obtain a third intermediate product; heating the third intermediate product from 1500° C. to 2500° C. at a rate of 10-12° C./min to realize atomic directional migration to obtain a fourth intermediate product; and heating the fourth intermediate product from 2500° C. to 2850° C., and keeping the fourth intermediate product at 2850° C. under an axial pulse pressure for 1-6 h to induce Bernal stacking to realize ordered lattice reconstruction, so as to obtain a fifth intermediate product; and
(S40) subjecting the fifth intermediate product to deagglomeration and magnetic separation to obtain a regenerated material.

### Claim 2 (depends on 1)

The method of claim 1, wherein in step (S20), the asphalt accounts for 5-10 wt. % of the pretreated waste layered carbon material.

### Claim 3 (depends on 1)

The method of claim 1, wherein the small-molecule aromatic hydrocarbons are anthracene and phenanthrene.

### Claim 4 (depends on 1)

The method of claim 1, wherein the defect sites are lattice vacancies and interlayer cracks.

### Claim 5 (depends on 1)

The method of claim 1, wherein in step (S20), the pyrolytic deposition is performed at a vacuum degree of 10−2 Pa.

### Claim 6 (depends on 1)

The method of claim 1, wherein the continuous carbon film has an amorphous-graphene hybrid structure with an intensity ratio of D-band to G-band (ID/IG ratio) of 0.45-0.55.

### Claim 7 (depends on 1)

The method of claim 1, wherein in step (S20), the isostatic-pressing densification is performed to increase a density of the continuous carbon film to 1.6-1.9 g/cm3.

### Claim 8 (depends on 1)

The method of claim 1, wherein during the defect identification and transformation, an oxygen-containing defect reaction is triggered as follows: C+O→CO2; a CO concentration is controlled at 300 ppm, and Stone Wales defect rotation is activated to realize transformation of five-membered carbon rings and seven-membered carbon rings into six-membered carbon rings.

### Claim 9 (depends on 1)

The method of claim 1, wherein during the atomic directional migration, under the guidance of the continuous carbon film, an atomic migration energy barrier is reduced, a vacancy filling energy barrier decreases by 1.3 eV, and an interlayer transition energy barrier decreases by 1.4 eV.

### Claim 10 (depends on 1)

The method of claim 1, wherein in step (S30), the axial pulse pressure is 0.4-0.55 MPa, and is applied in a 5-second on/5-second off mode.