# US 2026/0193811 A1 · Semi-insulating gallium arsenide single-crystal substrate, substrate with epitaxial layer, and method for manufacturing semi-insulating gallium arsenide single-crystal

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0193811 A1
- Document ID: US20260193811A1
- Status: Published application
- Kind: A1
- Application number: 19/128,587
- Filed: 2023-02-17
- Published: 2026-07-09
- Earliest claimed: 2023-02-17
- Assignees: Sumitomo Electric Industries, Ltd.
- Applicants: Sumitomo Electric Industries, Ltd.
- Inventors: Koichiro AOYAMA; Katsushi HASHIO; Tatsuya MORIWAKE; Masanori MORISHITA
- Web page: https://patentgrep.com/patent/US20260193811A1

## CPC

- C30B 29/42: Gallium arsenide
- B32B 3/02: characterised by features of form at particular places, e.g. in edge regions {(non-uniform thickness B32B3/263)}
- C30B 11/003: {Heating or cooling of the melt or the crystallised material}
- C30B 11/006: {Controlling or regulating}
- C30B 11/02: without using solvents (C30B11/06 takes precedence)
- C30B: SINGLE-CRYSTAL GROWTH (by using ultra-high pressure, e.g. for the formation of diamonds, B01J3/06); UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL (zone-refining of metals or alloys C22B); PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE (casting of metals, casting of other substances by the same processes or devices B22D; working of plastics B29; modifying the physical structure of metals or alloys C21D, C22F); SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE (for producing semiconductor devices or parts thereof H10); APPARATUS THEREFOR
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM

## Abstract

The semi-insulating gallium arsenide single-crystal substrate has a circular-shaped first main surface, in which a diameter of the semi-insulating gallium arsenide single-crystal substrate is 95 mm or more and 205 mm or less, a coefficient of light absorption of the semi-insulating gallium arsenide single-crystal substrate, with respect to near-infrared light at a wavelength of 940 nm, is 1.5 cm−1 or less, the number of etch pits per square centimeter, formed on the first main surface, in an etching test with immersion of the semi-insulating gallium arsenide single-crystal substrate in molten potassium hydroxide at 500° C. for 10 minutes is 300 or less, and a specific resistance of the semi-insulating gallium arsenide single-crystal substrate, as measured at 25° C. according to the Van der Pauw method, is 1.0×108 Ω·cm or more.

## Claims

### Claim 1

A semi-insulating gallium arsenide single-crystal substrate having a circular-shaped first main surface, wherein
a diameter of the semi-insulating gallium arsenide single-crystal substrate is 95 mm or more and 205 mm or less,
a coefficient of light absorption of the semi-insulating gallium arsenide single-crystal substrate, with respect to near-infrared light at a wavelength of 940 nm, is 1.5 cm−1 or less,
the number of etch pits per square centimeter, formed on the first main surface, in an etching test with immersion of the semi-insulating gallium arsenide single-crystal substrate in molten potassium hydroxide at 500° C. for 10 minutes is 300 or less, and
a specific resistance of the semi-insulating gallium arsenide single-crystal substrate, as measured at 25° C. in Hall measurement according to the Van der Pauw method, is 1.0×108 Ω·cm or more.

### Claim 2 (depends on 1)

The semi-insulating gallium arsenide single-crystal substrate according to claim 1, wherein the coefficient of light absorption is determined by applying the near-infrared light at a wavelength of 940 nm to the semi-insulating gallium arsenide single-crystal substrate at an angle of 85 degrees to measure a transmittance and a reflectance of the near-infrared light, of the semi-insulating gallium arsenide single-crystal substrate, with an ultraviolet-visible-infrared spectrophotometer, and assigning a numerical value of the transmittance and a numerical value of the reflectance, and a numerical value of a thickness of the semi-insulating gallium arsenide single-crystal substrate to the following expression 1, expression 2 and expression 3, and is determined together with a reflectance in one reflection of the near-infrared light in the semi-insulating gallium arsenide single-crystal substrate:
R
+
R
⁢
(
1
-
R
)
2
⁢
exp
⁡
(
-
2
⁢
α
⁢
d
)
/
(
1
-
r
)
=
R
*
Expression
⁢
1
(
1
-
R
)
2
⁢
exp
⁡
(
-
α
⁢
d
)
/
(
1
-
r
)
=
T
*
Expression
⁢
2
r
=
R
2
⁢
exp
⁡
(
2
⁢
α
⁢
d
)
Expression
⁢
3
wherein, in the expression 1, expression 2 and expression 3,
R* represents a reflectance in consideration of multiple reflections, as measured with the ultraviolet-visible-infrared spectrophotometer, and a unit of the reflectance is dimensionless,
T* represents a transmittance in consideration of multiple reflections, as measured with the ultraviolet-visible-infrared spectrophotometer, and a unit of the transmittance is dimensionless,
α represents the coefficient of light absorption, and a unit of the coefficient of light absorption is cm−1,
R represents a reflectance in one reflection of the near-infrared light in the semi-insulating gallium arsenide single-crystal substrate, and a unit of the reflectance in one reflection is dimensionless, and
d represents a thickness of the semi-insulating gallium arsenide single-crystal substrate, and a unit of the thickness is cm.

### Claim 3 (depends on 1)

The semi-insulating gallium arsenide single-crystal substrate according to claim 1, wherein
a carrier concentration in the semi-insulating gallium arsenide single-crystal substrate, as measured at 25° C. in Hall measurement according to the Van der Pauw method, is 8.0×106 cm−3 or less, and
an electron mobility of the semi-insulating gallium arsenide single-crystal substrate, as measured at 25° C. in Hall measurement according to the Van der Pauw method, is 4500 cm2/V·s or more.

### Claim 4 (depends on 1)

The semi-insulating gallium arsenide single-crystal substrate according to claim 1, wherein an average value of a residual strain, as an absolute value of a difference between a strain along a radial direction of the first main surface and a strain along a tangential direction of the first main surface, is 5.0×10−6 or less.

### Claim 5 (depends on 1)

The semi-insulating gallium arsenide single-crystal substrate according to claim 1, wherein an EL2 concentration of the semi-insulating gallium arsenide single-crystal substrate is 7.5×1015 cm−3 or more and 1.0×1016 cm−3 or less.

### Claim 6 (depends on 1)

The semi-insulating gallium arsenide single-crystal substrate according to claim 1, wherein
the semi-insulating gallium arsenide single-crystal substrate contains carbon, and
an atomic concentration of the carbon in the semi-insulating gallium arsenide single-crystal substrate is 5.0×1015 cm−3 or more and 1.2×1016 cm−3 or less.

### Claim 7 (depends on 1)

The semi-insulating gallium arsenide single-crystal substrate according to claim 1, to be used in a vertical cavity surface emitting laser.

### Claim 8 (depends on 1)

A substrate with an epitaxial layer, the substrate comprising the semi-insulating gallium arsenide single-crystal substrate according to claim 1, and an epitaxial layer placed on the first main surface, wherein
the epitaxial layer comprises an infrared emission layer.

### Claim 9

A method for manufacturing a semi-insulating gallium arsenide single crystal by use of a vertical boat method, the manufacturing method comprising
preparing a single crystal growth apparatus including at least a cylindrical crucible and a heating element that heats the crucible,
providing a seed crystal at a bottom portion of the crucible and providing gallium arsenide bulk at an upper portion as compared with the seed crystal in the crucible,
heating the crucible by the heating element to partially melt the gallium arsenide and the seed crystal, thereby not only obtaining a gallium arsenide melt, but also contacting the gallium arsenide melt and a residue of the seed crystal, and
growing a crystal on the seed crystal in the gallium arsenide melt to obtain a semi-insulating gallium arsenide single crystal, wherein
the obtaining a semi-insulating gallium arsenide single crystal is carried out with a relationship among the following formula 4, formula 5 and formula 6 being satisfied:
0.2
°C
.
/
⁢
mm
≤
X
≤
0.3
°C
.
/
⁢
mm
Formula
⁢
4
X
+
0.0012
°C
.
/
⁢
mm
2
×
Y
≤
Z
⁢
1
≤
X
+
0.0024
°C
.
/
⁢
mm
2
×
Y
Formula
⁢
5
0.26
°C
.
/
⁢
mm
≤
Z
⁢
2
≤
0.42
°C
.
/
⁢
mm
Formula
⁢
6
wherein, in the formula 4, formula 5 and formula 6,
X represents a temperature gradient along an axial direction of the crucible, as measured with, as a center, an interface between the crystal and the gallium arsenide melt, and a unit of the temperature gradient is ° C./mm,
Y represents a distance from the interface to a first reference point in the crystal, and a unit of the distance is mm,
Z1 represents a temperature gradient along an axial direction of the crucible, as measured with the first reference point as a center, and a unit of the temperature gradient is ° C./mm, and
Z2 represents a temperature gradient along an axial direction of the crucible, as measured with, as a center, the first reference point at a distance from the interface to the first reference point, of 50 mm, and a unit of the temperature gradient is ° C./mm.

### Claim 10 (depends on 9)

The method for manufacturing a semi-insulating gallium arsenide single crystal according to claim 9, wherein
the single crystal growth apparatus comprises one or more thermocouples outside in a radial direction of the crucible, and
position(s) of the thermocouple(s) is movable in a direction in parallel with an axial direction of the crucible.

### Claim 11 (depends on 2)

The semi-insulating gallium arsenide single-crystal substrate according to claim 2, wherein
a carrier concentration in the semi-insulating gallium arsenide single-crystal substrate, as measured at 25° C. in Hall measurement according to the Van der Pauw method, is 8.0×106 cm−3 or less,
an electron mobility of the semi-insulating gallium arsenide single-crystal substrate, as measured at 25° C. in Hall measurement according to the Van der Pauw method, is 4500 cm2/V·s or more,
an average value of a residual strain, as an absolute value of a difference between a strain along a radial direction of the first main surface and a strain along a tangential direction of the first main surface, is 5.0×10−6 or less,
an EL2 concentration of the semi-insulating gallium arsenide single-crystal substrate is 7.5×1015/cm−3 or more and 1.0×1016 cm−3 or less,
the semi-insulating gallium arsenide single-crystal substrate contains carbon, and
an atomic concentration of the carbon in the semi-insulating gallium arsenide single-crystal substrate is 5.0×1015 cm−3 or more and 1.2×1016 cm−3 or less.