# US 2026/0185257 A1 · Complexing agent and potassium chloride-based zinc-iron alloy plating solution containing the same, and zinc-iron electroplating method

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0185257 A1
- Document ID: US20260185257A1
- Status: Published application
- Kind: A1
- Application number: 19/420,567
- Filed: 2025-12-15
- Published: 2026-07-02
- Earliest claimed: 2024-12-30
- Assignees: Guangzhou Ultra Union Chemicals Ltd
- Applicants: Guangzhou Ultra Union Chemicals Ltd.
- Inventors: Chongwu GUO; FON VOON LAI; Xiaohua LI; Guifan FENG; Liang XIA
- Web page: https://patentgrep.com/patent/US20260185257A1

## CPC

- C25D 3/22: of zinc
- C23C 22/53: Treatment of zinc or alloys based thereon
- C23C 28/025: {with at least one zinc-based layer}
- C25D 3/565: {containing more than 50% by weight of zinc}
- C25D 5/48: After-treatment of electroplated surfaces
- C25D 17/12: Shape or form (C25D17/14 takes precedence)
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A complexing agent for zinc-iron alloy electroplating, including component A selected from the group consisting of sodium gluconate, sodium glucoheptonate, potassium sodium tartrate, sodium citrate and a combination thereof, component B being sodium sulfosalicylate. An electroplating solution is provided, including 50-70 g/L of zinc chloride, 2-12 g/L of ferrous chloride tetrahydrate, 160-240 g/L of potassium chloride, 25-35 g/L of boric acid, 6-55 g/L of the complexing agent, 0.1-0.2 mL/L of a brightener and 20-30 mL/L of an electroplating additive, with a pH of 4.5-5.6. During the electroplating process, a temperature of a plating bath is controlled at 15-30° C., a cathode current density is 1-3 A/dm2 and a swept rate of cathode is 3-5 m/min.

## Claims

### Claim 1

A complexing agent for a potassium chloride-based zinc-iron alloy plating solution, comprising:
a component A; and
a component B;
wherein the component A is selected from the group consisting of sodium gluconate, sodium glucoheptonate, potassium sodium tartrate, sodium citrate and a combination thereof;
the component B is sodium sulfosalicylate;
a weight ratio of the component A to the component B is 3:1-3; and
a weight concentration of the complexing agent in the potassium chloride-based zinc-iron alloy plating solution is 6-55 g/L.

### Claim 2

A potassium chloride-based zinc-iron alloy plating solution, comprising:
50-70. g/L of zinc chloride;
2-12. g/L of ferrous chloride tetrahydrate or 3-17 g/L of ferrous sulfate heptahydrate;
160-240. g/L of potassium chloride;
25-35. g/L of boric acid;
6-55. g/L of a complexing agent;
0.1-0.2 mL/L of a brightener; and
20-30. mL/L of an electroplating additive;
wherein the potassium chloride-based zinc-iron alloy plating solution has a pH of 4.5-5.6; and
the complexing agent comprises a component A and a component B; the component A is selected from the group consisting of sodium gluconate, sodium glucoheptonate, potassium sodium tartrate, sodium citrate and a combination thereof;
the component B is sodium sulfosalicylate; and the component A and the component B are mixed according to a weight ratio of 3:1-3.

### Claim 3 (depends on 2)

The potassium chloride-based zinc-iron alloy plating solution of claim 2, wherein the brightener comprises o-chlorobenzaldehyde and formic acid in a weight ratio of 1:0.8-1.2; and
the electroplating additive comprises 17-23 parts by weight of a sulfonation product of a fatty alcohol polyoxyethylene ether and sulfamic acid, 5-7 parts by weight of sodium benzoate, 0.4-0.6 part by weight of nicotinic acid and 80-90 parts by weight of water.

### Claim 4 (depends on 2)

The potassium chloride-based zinc-iron alloy plating solution of claim 2, wherein the brightener is prepared through steps of:
mixing o-chlorobenzaldehyde with formic acid in the weight ratio of 1:0.8-1.2 under stirring to obtain the brightener.

### Claim 5 (depends on 2)

The potassium chloride-based zinc-iron alloy plating solution of claim 2, wherein the electroplating additive is prepared through steps of:
adding 17-23 kg of the sulfonation product, 5-7 kg of sodium benzoate and 0.4-0.6 kg of nicotinic acid to 70 kg of water, followed by stirring for complete dissolution and dilution to 100 L with water, so as to obtain the electroplating additive.

### Claim 6 (depends on 2)

The potassium chloride-based zinc-iron alloy plating solution of claim 2, wherein the potassium chloride-based zinc-iron alloy plating solution is prepared through steps of:
adding water to a plating bath followed by addition of zinc chloride, potassium chloride, boric acid, and the complexing agent and stirring for dissolution, wherein the water added to the plating bath is 70% of a predetermined volume of the potassium chloride-based zinc-iron alloy plating solution;
adding ferrous chloride tetrahydrate to the plating bath followed by stirring for dissolution;
adding the brightener and the electroplating additive to the plating bath followed by stirring, adjustment to pH 4.5-5.6 with a 10 wt. % sodium hydroxide solution or a 3 wt. % hydrochloric acid solution, and addition of water to the predetermined volume to produce a mixture; and
electrolyzing the mixture at a current density of 0.1-0.2 A/dm2 for 30-90 minutes to produce the potassium chloride-based zinc-iron alloy plating solution.

### Claim 7 (depends on 2)

A zinc-iron electroplating method, comprising:
preparing the potassium chloride-based zinc-iron alloy plating solution of claim 2;
preprocessing a workpiece;
in the potassium chloride-based zinc-iron alloy plating solution, electroplating zinc-iron alloy on a preprocessed workpiece to give an electroplated workpiece;
subjecting the electroplated workpiece to trivalent chromium passivation to form a passivation film-coated workpiece; and
sealing the passivation film-coated workpiece with a graphene-modified sealant to form a graphene-modified sealing film, thereby obtaining a finished workpiece;
wherein a temperature of a plating bath is controlled at 15-30° C., a current density of a cathode is 1-3 A/dm2, and a swept rate of cathode is 3-5 m/min.

### Claim 8 (depends on 7)

The zinc-iron electroplating method of claim 7, wherein an anode is a zinc plate with a weight percentage of 99.99%.

### Claim 9 (depends on 7)

The zinc-iron electroplating method of claim 7, wherein an area ratio of a cathode to an anode is 2:0.7-1.3.

### Claim 10 (depends on 7)

The zinc-iron electroplating method of claim 7, wherein a 30 wt. % ferrous chloride tetrahydrate solution is supplemented to the plating bath during production, so as to maintain a weight concentration of ferrous chloride tetrahydrate at 2-12 g/L.