# US 2026/0158755 A1 · Glass cover manufacturing using a single-crystal silicon mold

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0158755 A1
- Document ID: US20260158755A1
- Status: Published application
- Kind: A1
- Application number: 19/049,953
- Filed: 2025-02-10
- Published: 2026-06-11
- Earliest claimed: 2024-02-16
- Assignees: Murata Manufacturing Co., Ltd.
- Applicants: Murata Manufacturing Co., Ltd.
- Inventors: Jaakko RUOHIO; Anssi BLOMQVIST; Mikael KAUTTO
- Web page: https://patentgrep.com/patent/US20260158755A1

## CPC

- B29D 11/00307: {Producing lens wafers}
- B81C 1/00317: {Packaging optical devices}
- C03B 23/02: Re-forming glass sheets
- C03B 23/0355: {by blowing without suction directly on the glass sheet}
- C03B 23/0357: {by suction without blowing, e.g. with vacuum or by venturi effect}
- G02B 26/0833: {the reflecting element being a micromechanical device, e.g. a MEMS mirror, DMD (G02B26/0825 takes precedence; micromechanical devices in general B81B)}
- B81B 2201/042: Micromirrors, not used as optical switches
- B81B 2203/0384: sloped profile
- B81C 2201/0133: Wet etching
- B29D: PRODUCING PARTICULAR ARTICLES FROM PLASTICS OR FROM SUBSTANCES IN A PLASTIC STATE (making granules B29B9/00; making preforms B29B11/00)
- B81C: PROCESSES OR APPARATUS SPECIALLY ADAPTED FOR THE MANUFACTURE OR TREATMENT OF MICROSTRUCTURAL DEVICES OR SYSTEMS (making microcapsules or microballoons B01J13/02; processes or apparatus specially adapted for the manufacture or treatment of piezoelectric, electrostrictive or magnetostrictive elements per se H10N30/01)
- C03B: MANUFACTURE, SHAPING, OR SUPPLEMENTARY PROCESSES
- G02B: OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
- B81B: MICROSTRUCTURAL DEVICES OR SYSTEMS, e.g. MICROMECHANICAL DEVICES (piezoelectric, electrostrictive or magnetostrictive elements per se H10N30/00, H10N35/00)

## Abstract

The disclosure relates to methods of manufacturing a plurality of devices having an optical glass cover comprising an angled optical window. An off-axis cut silicon wafer is used as a mold for molding borosilicate glass to form a plurality of angled glass portions. The polished borosilicate glass is anodically bonded to a silicon device wafer comprising a plurality of structures or circuitry for the plurality of devices. After removing the silicon mold by etching, the silicon wafer stack is diced to separate the plurality of devices, each having the optical glass cover comprising a respective angled optical window determined by one of the angled recesses of the silicon mold.

## Claims

### Claim 1

A method of manufacturing a plurality of devices having an optical glass cover comprising an angled optical window, the method comprises:
patterning a face of an off-axis cut silicon wafer to determine a plurality of unmasked areas of the off-axis cut silicon wafer;
wet-etching the plurality of unmasked areas to reveal a plurality of Si surfaces of the off-axis cut silicon wafer, to form a silicon mold comprising a plurality of angled recesses, wherein an angled shape of each angled recess is determined by a respective Si surface;
molding heat-softened borosilicate glass using the silicon mold to form a plurality of angled glass portions;
cooling the molded borosilicate glass;
polishing the cooled borosilicate glass;
anodically bonding the polished borosilicate glass to a silicon device wafer comprising a plurality of structures or circuitry for the plurality of devices;
removing the silicon mold by etching to release a wafer stack with the borosilicate glass and the silicon device wafer; and
dicing the wafer stack to separate the plurality of devices having the optical glass cover,
wherein the optical glass cover of each device comprises the respective angled optical window determined by one of the angled recesses of the silicon mold.

### Claim 2 (depends on 1)

The method of manufacturing according to claim 1, further comprising improving a quality of the plurality of Si surfaces by hydrogen (H2) or acid treatment.

### Claim 3 (depends on 1)

The method of manufacturing according to claim 1, further comprising removing the silicon mold by ethylene diamine pyrocatechol (EDP) etching or by reactive-ion etching (RIE).

### Claim 4 (depends on 1)

The method according to claim 1, wherein molding the borosilicate glass using the silicon mold further comprises:
applying a sheet of borosilicate glass on the silicon mold in vacuum to hermetically seal the plurality of angled recesses in the silicon mold, and
a) heating up the sheet of borosilicate glass, and applying an inert pressure to cause the heated sheet of borosilicate glass to adapt to the shape of the silicon mold, or
b) heating up the sheet of borosilicate glass into a temperature above its Littleton Softening Point and allowing the heated sheet of borosilicate glass to adapt to the shape of the silicon mold under its own weight.

### Claim 5 (depends on 4)

The method according to claim 4, wherein a thickness of the sheet of borosilicate glass is less than a greatest vertical distance from non-etched portions of the patterned face of the silicon mold to a bottom of the recess formed by the angled portion of the silicon mold.

### Claim 6 (depends on 5)

The method according to claim 5, wherein the thickness of the sheet of borosilicate glass is between 50 μm and 500 μm.

### Claim 7 (depends on 1)

The method according to claim 1, wherein molding the borosilicate glass using the silicon mold comprises:
molding a layer of heat-softened borosilicate glass on the silicon mold, and
grinding the molded layer of borosilicate glass after cooling and before polishing.

### Claim 8 (depends on 6)

The method according to claim 6, wherein a thickness of a layer of borosilicate glass is more than a greatest vertical distance from non-etched portions of the patterned face of the silicon mold to the bottom of the recess formed by the angled portion of the silicon mold.

### Claim 9 (depends on 7)

The method according to claim 7, wherein a thickness of the layer of borosilicate glass is between 200 μm and 1000 μm.

### Claim 10 (depends on 1)

The method according to claim 1, wherein a cut angle (α) of the off-axis cut silicon wafer is in a range from 5° to 25° with respect to a Si crystal orientation, and a tilt angle (β) of the angled optical window is equal to the cut angle (α) of the off-axis cut silicon wafer.

### Claim 11 (depends on 1)

The method according to claim 1, wherein the plurality of structures or devices comprise a plurality of MEMS devices.

### Claim 12 (depends on 1)

The method according to claim 1, wherein the plurality of structures or devices comprise a plurality of MEMS mirrors, and wherein the cut angle (α) of the off-axis cut silicon wafer is greater than maximum tilt angle (β) of the respective MEMS mirror.

### Claim 13 (depends on 1)

A MEMS mirror manufactured using the method according to claim 1.

### Claim 14 (depends on 12)

A pair of augmented reality (AR) glasses, a pair of virtual reality (VR) glasses or a heads-up display comprising at least one MEMS mirror according to claim 12.

### Claim 15

A method of manufacturing a plurality of devices having an optical glass cover comprising an angled optical window, the method comprises:
patterning a face of an off-axis cut silicon wafer to determine a plurality of unmasked areas of the off-axis cut silicon wafer;
wet-etching the plurality of unmasked areas to reveal a plurality of Si surfaces of the off-axis cut silicon wafer, to form a silicon mold comprising a plurality of angled recesses, wherein an angled shape of each angled recess is determined by a respective Si surface;
molding heat-softened borosilicate glass using the silicon mold to form a plurality of angled glass portions;
cooling the molded borosilicate glass;
polishing the cooled borosilicate glass;′
anodically bonding the polished borosilicate glass to a silicon device wafer comprising a plurality of structures or circuitry for the plurality of devices; and
dicing a wafer stack to separate the plurality of devices having the optical glass cover, wherein the optical glass cover of each device comprises the respective angled optical window determined by one of the angled recesses of the silicon mold,
wherein thickness of a layer of borosilicate glass is between 50 μm and 500 μm, and
wherein the thickness of the layer of borosilicate glass is more than a greatest vertical distance from non-etched portions of the patterned face of the silicon mold to a bottom of the recess formed by the angled portion of the silicon mold.

### Claim 16 (depends on 15)

The method according to claim 15, wherein the molding of the borosilicate glass using the silicon mold further comprises:
applying the layer of borosilicate glass on the silicon mold in vacuum to hermetically seal the plurality of angled recesses in the silicon mold, and
a) heating up the layer of borosilicate glass, and applying an inert pressure to cause the heated layer of borosilicate glass to adapt to the shape of the silicon mold, or
b) heating up the layer of borosilicate glass into a temperature above its Littleton Softening Point and allowing a heated sheet of borosilicate glass to adapt to the shape of the silicon mold under its own weight.

### Claim 17 (depends on 16)

The method according to claim 16, wherein a thickness of the layer of borosilicate glass is less than a greatest vertical distance from non-etched portions of the patterned face of the silicon mold to a bottom of the recess formed by the angled portion of the silicon mold.

### Claim 18 (depends on 15)

The method according to claim 15, wherein molding the borosilicate glass using the silicon mold comprises:
molding a layer of heat-softened borosilicate glass on the silicon mold; and
grinding the molded layer of borosilicate glass after cooling and before polishing.

### Claim 19

A method of manufacturing a plurality of devices having an optical glass cover comprising an angled optical window, the method comprises:
patterning a face of an off-axis cut silicon wafer to determine a plurality of unmasked areas of the off-axis cut silicon wafer;
wet-etching the plurality of unmasked areas to reveal a plurality of Si surfaces of the off-axis cut silicon wafer to form a silicon mold comprising a plurality of angled recesses, wherein an angled shape of each angled recess is determined by a respective Si surface;
molding a heat-softened borosilicate glass using the silicon mold to form a plurality of angled glass portions;
cooling the molded borosilicate glass;
polishing the cooled borosilicate glass;
anodically bonding the polished borosilicate glass to a silicon device wafer comprising a plurality of structures or circuitry for the plurality of devices; and
removing the silicon mold by etching to release a wafer stack with the borosilicate glass and the silicon device; and
dicing a wafer stack to separate the plurality of devices having the optical glass cover, wherein the optical glass cover of each device comprises the respective angled optical window determined by one of the angled recesses of the silicon mold;
wherein molding borosilicate glass using the silicon mold further comprises:
molding a layer of heat-softened borosilicate glass on the silicon mold, and
grinding the molded layer of borosilicate glass after cooling and before polishing, and
wherein thickness of the layer of borosilicate glass is between 200 μm and 1000 μm.

### Claim 20 (depends on 19)

The method according to claim 19, wherein cooling of the molded borosilicate glass is performed using a controlled temperature ramp to ensure high quality of the borosilicate glass.