# US 2026/0146305 A1 · Nanoparticle Dispersion Strengthened Copper Alloy and Preparation Method and Use Thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0146305 A1
- Document ID: US20260146305A1
- Status: Published application
- Kind: A1
- Application number: 18/729,247
- Filed: 2023-05-29
- Published: 2026-05-28
- Earliest claimed: 2023-01-16
- Assignees: Central South University
- Applicants: Central South University
- Inventors: Zhou Li; Wenting Qiu; Zhu Xiao
- Web page: https://patentgrep.com/patent/US20260146305A1

## CPC

- C22C 1/059: Making alloys comprising less than 5% by weight of dispersed reinforcing phases
- C22C 1/0425: {Copper-based alloys}
- C22C 1/057: with in situ formation of phases other than hard compounds by solid state reaction sintering, e.g. metal phase formed by reduction reaction
- C22C 9/00: Alloys based on copper
- C22C 32/0021: {Matrix based on noble metals, Cu or alloys thereof}
- C22F 1/08: of copper or alloys based thereon
- C22C 1/1078: {by internal oxidation of material in solid state}
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

The present disclosure relates to a nanoparticle dispersion strengthened copper alloy and a preparation method and use thereof. The method includes the steps of: S1) preparing Cu—Al2O3 dispersed copper powder from Cu—Al alloy powder by internal oxidation and reduction; and S2) mixing the Cu—Al2O3 dispersed copper powder prepared in S1 with Cr powder to obtain a composite powder, and subjecting the composite powder to press forming, hot press sintering, sheath moulding, and then aging treatment, where the hot press sintering is conducted at a temperature of 900° C. to 1070° C. and a pressure of 40 MPa to 80 MPa for 2 hours to 8 hours.

## Claims

### Claim at position 1

1-10. (canceled)

### Claim 11

A method for preparing a nanoparticle dispersion strengthened copper alloy, comprising the steps of:
S1: preparing Cu—Al2O3 dispersed copper powder from Cu—Al alloy powder by internal oxidation and reduction; and
S2: mixing the Cu—Al2O3 dispersed copper powder prepared in step S1 with Cr powder to obtain a composite powder, and subjecting the composite powder to press forming, hot press sintering, sheath moulding, hot extrusion, solid solution treatment, cold deformation, and then aging treatment;
wherein the hot press sintering is conducted at a temperature within an approximate range of 900° C. to 1070° C. and a pressure within an approximate range of 40 MPa to 80 MPa for a duration within an approximate range of 2 hours to 8 hours.

### Claim 12 (depends on 11)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 11, wherein
the main components of the nanoparticle dispersion strengthened copper alloy are copper, Al2O3 and Cr, wherein
the nanoparticle dispersion strengthened copper alloy contains Al2O3 in a range of 0.23 vol % to 4.5 vol % and Cr in a range of 0.05 wt % to 5 wt %.

### Claim 13 (depends on 11)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 11, wherein the internal oxidation includes the steps of:
melting Al and Cu at 1200° C. to 1230° C. to prepare the alloy powder by atomization using a protective gas, and then
mixing the resulting alloy powder with an oxidizing agent for oxidation reaction, wherein the oxidizing agent is at least one of Cu2O and CuO.

### Claim 14 (depends on 13)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 13, wherein a mass ratio of the oxidizing agent to the alloy powder ranges from 0.005:1 to 10:1.

### Claim 15 (depends on 13)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 13, wherein the protective gas is nitrogen or inert gas.

### Claim 16 (depends on 13)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 13, wherein the internal oxidation further includes the step of sieving the alloy powder obtained by atomization to sieve out the alloy powder with a particle size of less than 40 mesh.

### Claim 17 (depends on 16)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 16, wherein the internal oxidation is conducted at a temperature ranging from 880° C. to 920° C. for a duration ranging from 1 hour to 8 hours.

### Claim 18 (depends on 11)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 11, wherein the reduction includes crushing the alloy powder obtained by the internal oxidation and then conducting the reduction.

### Claim 19 (depends on 18)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 18, wherein the reduction is conducted by hydrogen reduction at 800° C. to 900° C. for 2 hours to 8 hours.

### Claim 20 (depends on 11)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 11, wherein the hot extrusion is conducted at a temperature ranging from 880° C. to 920° C. and at an extrusion ratio no less than 8:1.

### Claim 21 (depends on 11)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 11, wherein the aging treatment is conducted at a temperature within an approximate range of 400° C. to 500° C. for a duration within an approximate range of 1 hour to 10 hours.

### Claim 22 (depends on 11)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 11, wherein the composite powder contains Al2O3 in a range of 0.27 vol % to 4.5 vol % and Cr in a range of 0.05 wt % to 5 wt %.

### Claim 23 (depends on 13)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 13, wherein the oxidizing agent and the alloy powder are mixed at a ratio where the ratio of the oxygen in the oxidizing agent to the aluminum in the powder, O:Al, ranges from 0.9:1 to 1.8:1.

### Claim 24 (depends on 11)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 11, wherein the hot extrusion is conducted at a temperature ranging from 900° C. to 920° C.

### Claim 25 (depends on 11)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 11, wherein the solid solution treatment is conducted at a temperature ranging from 920° C. to 1050° C. for a duration ranging from 2 hours to 8 hours, and water-quenching is conducted after the solid solution treatment.

### Claim 26 (depends on 11)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 11, wherein the cold deformation is conducted to a ratio ranging from 60% to 85%.

### Claim 27 (depends on 11)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 11, wherein the cold deformation includes cold forging or cold drawing.

### Claim 28 (depends on 27)

The method for preparing a nanoparticle dispersion strengthened copper alloy according to claim 27, wherein the cold forging is rotary forging.

### Claim 29 (depends on 11)

A nanoparticle dispersion strengthened copper alloy prepared according to the method of claim 11.