# US 2026/0117097 A1 · Flame-retardant degradable adhesive tape and preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0117097 A1
- Document ID: US20260117097A1
- Status: Published application
- Kind: A1
- Application number: 18/294,384
- Filed: 2022-03-23
- Published: 2026-04-30
- Earliest claimed: 2022-03-18
- Assignees: Shanghai University of Engineering Science
- Applicants: Shanghai University of Engineering Science
- Inventors: Zhenlin JIANG; Yun ZHANG; Keyu ZHU; Chenxue XU; Min ZHU; Xin FAN; Jiamin XU; Wanting REN
- Web page: https://patentgrep.com/patent/US20260117097A1

## CPC

- C09J 7/255: {Polyesters}
- C09J 7/38: Pressure-sensitive adhesives [PSA]
- C09J 167/00: Adhesives based on polyesters obtained by reactions forming a carboxylic ester link in the main chain (based on polyester-amides C09J177/12; based on polyester-imides C09J179/08); Adhesives based on derivatives of such polymers
- C09J 167/06: Unsaturated polyesters having carbon-to-carbon unsaturation
- C08G 63/183: Terephthalic acids
- C08G 63/6926: {Dicarboxylic acids and dihydroxy compounds}
- C08G 63/916: {Dicarboxylic acids and dihydroxy compounds}
- C09J 2301/302: the adhesive being pressure-sensitive, i.e. tacky at temperatures inferior to 30°C
- C09J 2301/408: additives as essential feature of the adhesive layer
- C09J 2301/414: presence of a copolymer
- C09J 2467/00: Presence of polyester
- C09J 2467/006: in the substrate
- C09J: ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES (preparation of glue or gelatine C09H)
- C08G: MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS

## Abstract

The present disclosure provides a preparation method of a flame-retardant degradable adhesive tape, including: preparing a degradable adhesive tape base layer and a flame-retardant degradable adhesive tape bonding layer separately, and then conducting coating, curing, and aging of the flame-retardant degradable adhesive tape bonding layer on a surface of the degradable adhesive tape base layer to obtain the flame-retardant degradable adhesive tape; where the degradable adhesive tape base layer is prepared by subjecting bis(2-hydroxybutyl) terephthalate (BHBT) and bis(2-hydroxybutyl) adipate (BHAT) to transesterification and polycondensation to obtain a degradable poly(butylene adipate-co-terephthalate) (PBAT) polymer polymer, and then conducting blow molding on the degradable PBAT polymer; the flame-retardant degradable adhesive tape bonding layer is prepared by subjecting the BHBT, the BHAT, and a pressure-sensitive adhesive (PSA) additive to transesterification and polycondensation to obtain a colloidal flame-retardant degradable PBAT polymer, and conducting curing on the colloidal flame-retardant degradable PBAT polymer.

## Claims

### Claim 1

A preparation method of a flame-retardant degradable adhesive tape, comprising: preparing a degradable adhesive tape base layer and a flame-retardant degradable adhesive tape bonding layer separately, and then conducting coating, curing, and aging of the flame-retardant degradable adhesive tape bonding layer on a surface of the degradable adhesive tape base layer to obtain the flame-retardant degradable adhesive tape; wherein the degradable adhesive tape base layer is prepared by subjecting bis(2-hydroxybutyl) terephthalate (BHBT) and bis(2-hydroxybutyl) adipate (BHAT) to transesterification and polycondensation to obtain a degradable poly(butylene adipate-co-terephthalate) (PBAT) polymer, and then conducting blow molding on the degradable PBAT polymer;
the flame-retardant degradable adhesive tape bonding layer is prepared by subjecting the BHBT, the BHAT, and a pressure-sensitive adhesive (PSA) additive to transesterification and polycondensation to obtain a colloidal flame-retardant degradable PBAT polymer, and conducting curing on the colloidal flame-retardant degradable PBAT polymer; and
the PSA additive is prepared by conducting esterification on 2-carboxyethylphenylphosphinic acid (CEPPA), 1,4-butanediol, and pentaerythritol.

### Claim 2 (depends on 1)

The preparation method of a flame-retardant degradable adhesive tape according to claim 1, wherein a process of conducting the coating, the curing, and the aging of the flame-retardant degradable adhesive tape bonding layer on the surface of the degradable adhesive tape base layer to obtain the flame-retardant degradable adhesive tape specifically comprises: coating the flame-retardant degradable adhesive tape bonding layer on the surface of the degradable adhesive tape base layer, conducting the curing by baking at 85° C. to 95° C. for 2 min to 4 min, laying a release film on a surface of the flame-retardant degradable adhesive tape bonding layer, and conducting the aging in a warm room at 45° C. to 55° C. for 23 h to 25 h to obtain the flame-retardant degradable adhesive tape; wherein
the release film is an organic silicone oil material;
the release film has a thickness of 0.1 μm to 8 μm;
the degradable adhesive tape base layer has a thickness of 10 μm to 60 μm; and
the flame-retardant degradable adhesive tape bonding layer has a thickness of 3 μm to 50 μm.

### Claim 3 (depends on 1)

The preparation method of a flame-retardant degradable adhesive tape according to claim 1, wherein the BHBT is regenerated BHBT prepared by conducting alcoholysis and filtration on a waste polybutylece terephthalate (PBT) material as a raw material;
the alcoholysis is conducted with sodium phytate or potassium phytate as a complexant; and
the regenerated BHBT has a residual metal ion content of less than 30 ppm.

### Claim 4 (depends on 3)

The preparation method of a flame-retardant degradable adhesive tape according to claim 3, wherein the waste PBT material has polyurethane (PU) with a mass fraction of less than 5% and polyethylene terephthalate (PET) with a mass fraction of less than 10%.

### Claim 5 (depends on 3)

The preparation method of a flame-retardant degradable adhesive tape according to claim 3, wherein the alcoholysis comprises: under nitrogen protection, dissolving the waste PBT material, the 1,4-butanediol, a catalyst, an anti-aging agent, and an ether inhibitor in a reactor at 180° C. to 210° C. to obtain a system; after the system is clarified, gradually heating to 200° C. to 240° C. to allow a reaction for 1.5 h to 2.5 h; recording a water output, and conducting vacuumizing at a vacuum degree of 200 Pa to 1,000 Pa for 20 min to 60 min when the water output reaches 90% of a theoretical value; and adding the complexant to allow a reaction for 15 min to 30 min, and conducting filtration to obtain the regenerated BHBT; wherein
the waste PBT material and the 1,4-butanediol are at a mass ratio of 1:0.30 to 1:0.50;
the catalyst is selected from the group consisting of zinc acetate, aluminum acetate, and calcium acetate;
the catalyst has a mass 0.025 wt % to 0.15 wt % that of the waste PBT material;
the anti-aging agent is selected from the group consisting of triphenyl phosphate, trimethyl phosphite, and triethyl phosphite;
the anti-aging agent has a mass 0.075 wt % to 0.25 wt % that of the waste PBT material;
the ether inhibitor is selected from the group consisting of sodium acetate and magnesium acetate;
the ether inhibitor has a mass 0.1 wt % to 0.25 wt % that of the waste PBT material; and
the complexant has a mass 0.02 wt % to 0.05 wt % that of the waste PBT material.

### Claim 6 (depends on 5)

The preparation method of a flame-retardant degradable adhesive tape according to claim 5, wherein the waste PBT material is further subjected to a pretreatment before the alcoholysis; and the pretreatment comprises: processing the waste PBT material to obtain a PBT powder with a particle size of less than 2 mm, sieving, and drying a resulting sieved PBT powder in a vacuum oven at 100° C. to 130° C. for 8 h to 12 h.

### Claim 7 (depends on 1)

The preparation method of a flame-retardant degradable adhesive tape according to claim 1, wherein a preparation process of the BHAT comprises: under nitrogen protection, allowing adipic acid and the 1,4-butanediol with a molar ratio of 1:1.05 to 1:1.45 to have esterification in a reactor at 180° C. to 200° C. for 2 h to 4 h; recording a water output, and detecting an acid value when the water output reaches 90% of a theoretical value; and terminating the esterification when the acid value reaches 20 KOH mg/g to 40 KOH mg/g to obtain the BHAT.

### Claim 8 (depends on 1)

The preparation method of a flame-retardant degradable adhesive tape according to claim 1, wherein a preparation process of the PSA additive comprises: under nitrogen protection, conducting alcoholysis on the CEPPA, the 1,4-butanediol, a catalyst, an anti-aging agent, and an ether inhibitor in a reactor at 140° C. to 160° C.; after a resulting system is clarified, adding pentaerythritol to allow a reaction for 2 h to 4 h; gradually heating to 170° C. to 230° C. and recording a water output; and conducting vacuumizing at a vacuum degree of 300 Pa to 900 Pa for 30 min to 60 min when the water output reaches 90% of a theoretical value to obtain the PSA additive; wherein
the CEPPA and the 1,4-butanediol are at a molar ratio of 1:1.10 to 1:1.40;
the 1,4-butanediol and the pentaerythritol are at a molar ratio of 1:1.2 to 1:1.3;
the catalyst is selected from the group consisting of zinc acetate, aluminum acetate, and calcium acetate;
the catalyst has a mass 0.025 wt % to 0.15 wt % that of the CEPPa;
the anti-aging agent is selected from the group consisting of triphenyl phosphate, trimethyl phosphite, and triethyl phosphite;
the anti-aging agent has a mass 0.075 wt % to 0.25 wt % that of the CEPPA;
the ether inhibitor is selected from the group consisting of sodium acetate and magnesium acetate; and
the ether inhibitor has a mass 0.1 wt % to 0.25 wt % that of the CEPPA.

### Claim 9 (depends on 1)

The preparation method of a flame-retardant degradable adhesive tape according to claim 1, wherein a preparation process of the degradable adhesive tape base layer comprises:
(1) under nitrogen protection, dissolving the BHBT, the BHAT, and a condensation catalyst according a specified proportion in a reactor at 200° C. to 210° C. for 15 min, and gradually heating to 225° C. to 235° C. to allow a reaction for 1 h to 1.5 h; recording a water output, and heating to 250° C. to 265° C. to allow high-temperature polycondensation at a vacuum degree of 50 Pa to 1,000 Pa for 3.5 h to 5.5 h when the water output reaches 90% of a theoretical value, to obtain the degradable PBAT polymer; wherein
the BHBT and the BHAT are at a molar ratio of 40:60 to 50:50;
the condensation catalyst is a composite catalyst of poly(antimony ethylene glycoxide) and tetrabutyl titanate, and the poly(antimony ethylene glycoxide) and the tetrabutyl titanate are at a mass ratio of 1:0.25 to 1:0.85; and
the condensation catalyst is added at 0.01 wt % to 0.06 wt % of the BHAT; and
(2) subjecting the degradable PBAT polymer to blow molding at 160° C. to 180° C. and a blow-up ratio of (3-6):1 in a film blowing machine with a die gap of 10 μm to 50 μm, to obtain a regenerated PBAT polymer film as the degradable adhesive tape base layer.

### Claim 10 (depends on 1)

The preparation method of a flame-retardant degradable adhesive tape according to claim 1, wherein a preparation process of the flame-retardant degradable adhesive tape bonding layer comprises:
(1) under nitrogen protection, dissolving the BHBT, the BHAT, the PSA additive, and a condensation catalyst according a specified proportion in a reactor at 190° C. to 210° C. for 20 min, and gradually heating to 220° C. to 240° C. to allow a reaction for 1 h to 2 h; recording a water output, and heating to 245° C. to 250° C. to allow high-temperature polycondensation at a vacuum degree of 200 Pa to 600 Pa for 2.5 h to 4.5 h when the water output reaches 90% of a theoretical value, to obtain the colloidal flame-retardant degradable PBAT polymer; wherein
the BHBT, the BHAT, and the PSA additive are at a molar ratio of 35:50:15 to 20:50:30;
the condensation catalyst is a composite catalyst of poly(antimony ethylene glycoxide) and tetrabutyl titanate, and the poly(antimony ethylene glycoxide) and the tetrabutyl titanate are at a mass ratio of 1:0.25 to 1:0.85; and
the condensation catalyst is added at 0.01 wt % to 0.06 wt % of the BHAT; and
(2) aging the colloidal flame-retardant degradable PBAT polymer at 40° C. to 60° C., and allowing to stand for 1 h to 1.5 h to obtain the flame-retardant degradable adhesive tape bonding layer.

### Claim 11 (depends on 1)

A flame-retardant degradable adhesive tape prepared by the preparation method according to claim 1, comprising a degradable adhesive tape base layer and a flame-retardant degradable adhesive tape bonding layer; wherein
the degradable adhesive tape base layer has a tensile strength of greater than or equal to 20 MPa;
the flame-retardant degradable adhesive tape bonding layer has a number-average molecular weight of 6,000 to 12,000, a glass-transition temperature (GTT) of −25° C. to 0° C., a viscoelastic range of −25° C. to 72° C., a complex viscosity η* of 14 Pa·s to 30 Pa·s, an initial adhesion of greater than or equal to 20#, a permanent adhesion of greater than or equal to 30 h, and a 180° peel strength of greater than or equal to 5 N/cm under normal conditions; and
the flame-retardant degradable adhesive tape has a limiting oxygen index of 28% to 45%, a flame-retardant grade of UL94 VTM-0, and a 90-day biodegradation rate of 50% to 90%.

### Claim 12 (depends on 11)

The flame-retardant degradable adhesive tape according to claim 11, wherein a process of conducting the coating, the curing, and the aging of the flame-retardant degradable adhesive tape bonding layer on the surface of the degradable adhesive tape base layer to obtain the flame-retardant degradable adhesive tape specifically comprises: coating the flame-retardant degradable adhesive tape bonding layer on the surface of the degradable adhesive tape base layer, conducting the curing by baking at 85° C. to 95° C. for 2 min to 4 min, laying a release film on a surface of the flame-retardant degradable adhesive tape bonding layer, and conducting the aging in a warm room at 45° C. to 55° C. for 23 h to 25 h to obtain the flame-retardant degradable adhesive tape; wherein
the release film is an organic silicone oil material;
the release film has a thickness of 0.1 μm to 8 μm;
the degradable adhesive tape base layer has a thickness of 10 μm to 60 μm; and
the flame-retardant degradable adhesive tape bonding layer has a thickness of 3 μm to 50 μm.

### Claim 13 (depends on 11)

The flame-retardant degradable adhesive tape according to claim 11, wherein the BHBT is regenerated BHBT prepared by conducting alcoholysis and filtration on a waste polybutylece terephthalate (PBT) material as a raw material;
the alcoholysis is conducted with sodium phytate or potassium phytate as a complexant; and
the regenerated BHBT has a residual metal ion content of less than 30 ppm.

### Claim 14 (depends on 13)

The flame-retardant degradable adhesive tape according to claim 13, wherein the waste PBT material has polyurethane (PU) with a mass fraction of less than 5% and polyethylene terephthalate (PET) with a mass fraction of less than 10%.

### Claim 15 (depends on 13)

The flame-retardant degradable adhesive tape according to claim 13, wherein the alcoholysis comprises: under nitrogen protection, dissolving the waste PBT material, the 1,4-butanediol, a catalyst, an anti-aging agent, and an ether inhibitor in a reactor at 180° C. to 210° C. to obtain a system; after the system is clarified, gradually heating to 200° C. to 240° C. to allow a reaction for 1.5 h to 2.5 h; recording a water output, and conducting vacuumizing at a vacuum degree of 200 Pa to 1,000 Pa for 20 min to 60 min when the water output reaches 90% of a theoretical value; and adding the complexant to allow a reaction for 15 min to 30 min, and conducting filtration to obtain the regenerated BHBT; wherein
the waste PBT material and the 1,4-butanediol are at a mass ratio of 1:0.30 to 1:0.50;
the catalyst is selected from the group consisting of zinc acetate, aluminum acetate, and calcium acetate;
the catalyst has a mass 0.025 wt % to 0.15 wt % that of the waste PBT material;
the anti-aging agent is selected from the group consisting of triphenyl phosphate, trimethyl phosphite, and triethyl phosphite;
the anti-aging agent has a mass 0.075 wt % to 0.25 wt % that of the waste PBT material;
the ether inhibitor is selected from the group consisting of sodium acetate and magnesium acetate;
the ether inhibitor has a mass 0.1 wt % to 0.25 wt % that of the waste PBT material; and
the complexant has a mass 0.02 wt % to 0.05 wt % that of the waste PBT material.

### Claim 16 (depends on 15)

The flame-retardant degradable adhesive tape according to claim 15, wherein the waste PBT material is further subjected to a pretreatment before the alcoholysis; and the pretreatment comprises: processing the waste PBT material to obtain a PBT powder with a particle size of less than 2 mm, sieving, and drying a resulting sieved PBT powder in a vacuum oven at 100° C. to 130° C. for 8 h to 12 h.

### Claim 17 (depends on 11)

The flame-retardant degradable adhesive tape according to claim 11, wherein a preparation process of the BHAT comprises: under nitrogen protection, allowing adipic acid and the 1,4-butanediol with a molar ratio of 1:1.05 to 1:1.45 to have esterification in a reactor at 180° C. to 200° C. for 2 h to 4 h; recording a water output, and detecting an acid value when the water output reaches 90% of a theoretical value; and terminating the esterification when the acid value reaches 20 KOH mg/g to 40 KOH mg/g to obtain the BHAT.

### Claim 18 (depends on 11)

The flame-retardant degradable adhesive tape according to claim 11, wherein a preparation process of the PSA additive comprises: under nitrogen protection, conducting alcoholysis on the CEPPA, the 1,4-butanediol, a catalyst, an anti-aging agent, and an ether inhibitor in a reactor at 140° C. to 160° C.; after a resulting system is clarified, adding pentaerythritol to allow a reaction for 2 h to 4 h; gradually heating to 170° C. to 230° C. and recording a water output; and conducting vacuumizing at a vacuum degree of 300 Pa to 900 Pa for 30 min to 60 min when the water output reaches 90% of a theoretical value to obtain the PSA additive; wherein
the CEPPA and the 1,4-butanediol are at a molar ratio of 1:1.10 to 1:1.40;
the 1,4-butanediol and the pentaerythritol are at a molar ratio of 1:1.2 to 1:1.3;
the catalyst is selected from the group consisting of zinc acetate, aluminum acetate, and calcium acetate;
the catalyst has a mass 0.025 wt % to 0.15 wt % that of the CEPPa;
the anti-aging agent is selected from the group consisting of triphenyl phosphate, trimethyl phosphite, and triethyl phosphite;
the anti-aging agent has a mass 0.075 wt % to 0.25 wt % that of the CEPPA;
the ether inhibitor is selected from the group consisting of sodium acetate and magnesium acetate; and
the ether inhibitor has a mass 0.1 wt % to 0.25 wt % that of the CEPPA.

### Claim 19 (depends on 11)

The flame-retardant degradable adhesive tape according to claim 11, wherein a preparation process of the degradable adhesive tape base layer comprises:
(1) under nitrogen protection, dissolving the BHBT, the BHAT, and a condensation catalyst according a specified proportion in a reactor at 200° C. to 210° C. for 15 min, and gradually heating to 225° C. to 235° C. to allow a reaction for 1 h to 1.5 h; recording a water output, and heating to 250° C. to 265° C. to allow high-temperature polycondensation at a vacuum degree of 50 Pa to 1,000 Pa for 3.5 h to 5.5 h when the water output reaches 90% of a theoretical value, to obtain the degradable PBAT polymer; wherein
the BHBT and the BHAT are at a molar ratio of 40:60 to 50:50;
the condensation catalyst is a composite catalyst of poly(antimony ethylene glycoxide) and tetrabutyl titanate, and the poly(antimony ethylene glycoxide) and the tetrabutyl titanate are at a mass ratio of 1:0.25 to 1:0.85; and
the condensation catalyst is added at 0.01 wt % to 0.06 wt % of the BHAT; and
(2) subjecting the degradable PBAT polymer to blow molding at 160° C. to 180° C. and a blow-up ratio of (3-6):1 in a film blowing machine with a die gap of 10 μm to 50 μm, to obtain a regenerated PBAT polymer film as the degradable adhesive tape base layer.

### Claim 20 (depends on 11)

The flame-retardant degradable adhesive tape according to claim 11, wherein a preparation process of the flame-retardant degradable adhesive tape bonding layer comprises:
(1) under nitrogen protection, dissolving the BHBT, the BHAT, the PSA additive, and a condensation catalyst according a specified proportion in a reactor at 190° C. to 210° C. for 20 min, and gradually heating to 220° C. to 240° C. to allow a reaction for 1 h to 2 h; recording a water output, and heating to 245° C. to 250° C. to allow high-temperature polycondensation at a vacuum degree of 200 Pa to 600 Pa for 2.5 h to 4.5 h when the water output reaches 90% of a theoretical value, to obtain the colloidal flame-retardant degradable PBAT polymer; wherein
the BHBT, the BHAT, and the PSA additive are at a molar ratio of 35:50:15 to 20:50:30;
the condensation catalyst is a composite catalyst of poly(antimony ethylene glycoxide) and tetrabutyl titanate, and the poly(antimony ethylene glycoxide) and the tetrabutyl titanate are at a mass ratio of 1:0.25 to 1:0.85; and
the condensation catalyst is added at 0.01 wt % to 0.06 wt % of the BHAT; and
(2) aging the colloidal flame-retardant degradable PBAT polymer at 40° C. to 60° C., and allowing to stand for 1 h to 1.5 h to obtain the flame-retardant degradable adhesive tape bonding layer.