# US 2026/0107749 A1 · Superconformal molybdenum via fill by use of deposition gradient control

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0107749 A1
- Document ID: US20260107749A1
- Status: Published application
- Kind: A1
- Application number: 18/916,446
- Filed: 2024-10-15
- Published: 2026-04-16
- Earliest claimed: 2024-10-15
- Applicants: Applied Materials, Inc.
- Inventors: Jiajie CEN; Wenting HOU; Shiyu YUE; Shiyu HU; Ruinan ZHOU; Rongjun WANG; Xianmin TANG
- Web page: https://patentgrep.com/patent/US20260107749A1

## CPC

- C23C 16/045: {Coating cavities or hollow spaces, e.g. interior of tubes; Infiltration of porous substrates}
- H10W 20/056: {by filling conductive material into holes, grooves or trenches}
- C23C 16/0281: {of metallic sub-layers (C23C16/029 takes precedence)}
- C23C 16/14: Deposition of only one other metal element
- H10P 14/432: {using selective deposition}
- H10W 20/033: {in openings in dielectrics}
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- H10W: GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
- H10P: GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10

## Abstract

The present disclosure provides metal gap fill deposition methods on a semiconductor substrate. The methods include forming a liner layer on a surface of a feature by providing a first dosage and a second dosage of a first metal-containing precursor to a processing chamber. The feature includes a feature formed in a surface of the semiconductor substrate. The feature includes an opening that is defined by a capping layer and side walls. The side walls include a dielectric material. The liner layer is formed over the side walls and the capping layer. A metal gap fill material is deposited over the liner layer to fill the feature formed in the surface of the semiconductor substrate by providing a second metal-containing precursor and a hydrogen-containing precursor to the processing chamber.

## Claims

### Claim 1

A method of metal gap fill deposition on a semiconductor substrate, comprising:
forming a liner layer on a surface of a feature by providing a first dosage and a second dosage of a first metal-containing precursor to a processing chamber, wherein:
the feature comprises a feature formed in a surface of the semiconductor substrate,
the feature comprises an opening that is defined by a capping layer and side walls, wherein the side walls comprise a dielectric material, and
the liner layer is formed over the side walls and the capping layer; and
depositing a metal gap fill material over the liner layer to fill the feature formed in the surface of the semiconductor substrate by providing a second metal-containing precursor and a hydrogen-containing precursor to the processing chamber.

### Claim 2 (depends on 1)

The method of claim 1, wherein the first dosage comprises introducing the first metal-containing precursor according to a chemical vapor deposition process, an atomic layer deposition process, or a molecular layer deposition process.

### Claim 3 (depends on 1)

The method of claim 1, wherein the second dosage comprises introducing the first metal-containing precursor according to a plasma enhanced deposition process.

### Claim 4 (depends on 3)

The method of claim 3, wherein the plasma enhanced deposition process comprises a plasma power of about 100 W to about 600 W.

### Claim 5 (depends on 1)

The method of claim 1, further comprising providing a first purge between the first dosage and the second dosage.

### Claim 6 (depends on 5)

The method of claim 5, further comprising providing a second purge after the second dosage.

### Claim 7 (depends on 6)

The method of claim 6, wherein the first dosage, the first purge, the second dosage, and the second purge are repeated for 400 to 1200 cycles.

### Claim 8 (depends on 1)

The method of claim 1, wherein the first metal-containing precursor is molybdenum oxychloride.

### Claim 9 (depends on 8)

The method of claim 8, wherein the second metal-containing precursor is molybdenum chloride and the hydrogen-containing precursor is H2.

### Claim 10 (depends on 1)

The method of claim 1, wherein the metal gap fill material comprises molybdenum.

### Claim 11 (depends on 1)

The method of claim 1, wherein depositing the metal gap fill material comprises depositing the metal gap fill material using an atomic layer deposition process or a chemical vapor deposition process.

### Claim 12 (depends on 1)

The method of claim 1, wherein depositing the metal gap fill material comprises:
delivering about 1 sccm to about 3000 sccm of the second metal-containing precursor to the processing chamber for a period of about 0.3 seconds(s) to about 1 second;
delivering a purge gas to the processing chamber for a period of about 1 s to about 2 s;
delivering about 5,000 sccm to about 30,000 sccm of the hydrogen-containing precursor to the processing chamber for a period of about 1 s to about 4 s; and
delivering the purge gas to the processing chamber for a period of about 1 s to about 2 s.

### Claim 13 (depends on 12)

The method of claim 12, further comprising repeating delivering the second metal-containing precursor, delivering the purge gas, and delivering the hydrogen-containing precursor for about 400 to 1200 cycles.

### Claim 14

A method of metal gap fill deposition on a semiconductor substrate, comprising:
forming a liner layer on a surface of a feature by providing a first dosage and a second dosage of a first metal-containing precursor comprising molybdenum oxychloride to a processing chamber, wherein:
the feature comprises a feature formed in a surface of the semiconductor substrate,
the feature comprises an opening that is defined by a capping layer and side walls, wherein the side walls comprise a dielectric material, and
the liner layer is formed over the side walls and the capping layer; and
depositing a metal gap fill material over the liner layer to fill the feature formed in the surface of the semiconductor substrate by providing a second metal-containing precursor comprising molybdenum chloride and a hydrogen-containing precursor comprising H2 to the processing chamber.

### Claim 15 (depends on 14)

The method of claim 14, wherein the first dosage comprises introducing the first metal-containing precursor according to a chemical vapor deposition process, an atomic layer deposition process, or a molecular layer deposition process.

### Claim 16 (depends on 14)

The method of claim 14, wherein the second dosage comprises introducing the first metal-containing precursor according to a plasma enhanced deposition process, wherein the plasma enhanced deposition process comprises a plasma power of about 100 W to about 600 W.

### Claim 17 (depends on 14)

The method of claim 14, further comprising:
providing a first purge between the first dosage and the second dosage; and
providing a second purge after the second dosage.

### Claim 18 (depends on 17)

The method of claim 17, wherein the first dosage, the first purge, the second dosage, and the second purge are repeated for 400 to 1200 cycles.

### Claim 19 (depends on 14)

The method of claim 14, wherein depositing the metal gap fill material comprises:
delivering 1 sccm to about 3000 sccm of the second metal-containing precursor to the processing chamber for a period of about 0.3 seconds(s) to about 1 second;
delivering a purge gas to the processing chamber for a period of about 1 s to about 2 s;
delivering about 5,000 sccm to about 30,000 sccm of the hydrogen-containing precursor to the processing chamber for a period of about 1 s to about 4 s; and
delivering the purge gas to the processing chamber for a period of about 1 s to about 2 s.

### Claim 20 (depends on 19)

The method of claim 19, further comprising repeating delivering the second metal-containing precursor, delivering the purge gas, and delivering the hydrogen-containing precursor for about 400 to 1200 cycles.