# US 2026/0101675 A1 · Low-magnetic-field gallium arsenide quantum hall resistance sample and preparation thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0101675 A1
- Document ID: US20260101675A1
- Status: Published application
- Kind: A1
- Application number: 18/900,904
- Filed: 2024-09-30
- Published: 2026-04-09
- Earliest claimed: 2023-10-17
- Assignees: Beijing Orient Institute of Measurement and Test
- Applicants: Beijing Orient Institute of Measurement and Test
- Inventors: Xiaoding Huang; Zhongwei Wang; Jianzhen Cai; Yang Wang; Yuqiao Huang; Yiping Zeng
- Web page: https://patentgrep.com/patent/US20260101675A1

## CPC

- H10N 52/85: Materials of the active region
- H10N 52/01: Manufacture or treatment
- H10N 52/101: {Semiconductor Hall-effect devices}
- Y02P 70/50: Manufacturing or production processes characterised by the final manufactured product
- H10N: ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A low-magnetic-field gallium arsenide Quantum Hall Resistance sample can reproduce a Quantum Hall Resistance effect under lower magnetic field conditions, and has a wider plateau width of the quantum resistance sample being equal or greater than 0.6 T, and the magnetic field condition corresponds to the central magnetic field of the plateau being 2 between 7 T and 8 T. The sample includes a GaAs heterojunction material, the GaAs heterojunction material has a seven-layer structure including first to seventh layers sequentially stacked upwards and bonded to a surface of a GaAs substrate. The first layer is a GaAs isolation layer, the second layer is GaAs/AlGaAs superlattice layer, the third layer is high-purity GaAs layer, the fourth layer is a two-dimensional electron gas layer, the fifth layer is an undoped AlxGa1-xAs isolation layer, the sixth layer is a Si-doped AlxGa1-xAs layer, and the seventh layer is a GaAs surface layer.

## Claims

### Claim 1

A low-magnetic-field gallium arsenide (GaAs) Quantum Hall Resistance sample, comprising:
a GaAs heterojunction material, wherein the GaAs heterojunction material has a seven-layer structure including first to seventh layers sequentially stacked upwards and bonded to a surface of a GaAs substrate;
wherein the first layer of the seven-layer structure is a GaAs isolation layer, the second layer of the seven-layer structure is gallium arsenide/aluminum gallium arsenide (GaAs/AlGaAs) superlattice layer, the third layer of the seven-layer structure is high-purity GaAs layer, the fourth layer of the seven-layer structure is a two-dimensional electron gas layer, the fifth layer of the seven-layer structure is an undoped AlxGa1-xAs isolation layer, the sixth layer of the seven-layer structure is a Si-doped AlxGa1-xAs layer, and the seventh layer of the seven-layer structure is a GaAs surface layer, and
wherein a thickness of the undoped AlxGa1-xAs isolation layer is in a range of 10 nanometers (nm) to 30 nm, and x is in a range of 0.28 to 0.32, to match a carrier concentration of the two-dimensional electron gas layer with an expected low magnetic field of a central magnetic field, which is positively related to the carrier concentration of the two-dimensional electron gas layer, of a Quantum Hall Resistance plateau 2, and also to match the carrier concentration of the two-dimensional electron gas layer with an expected lower limit of a plateau width, which is positively related to the carrier concentration of the two-dimensional electron gas layer, of the Quantum Hall Resistance plateau 2; and the low magnetic field is in a range of 7 tesla (T) to 8 T, and the plateau width of the Quantum Hall Resistance plateau 2 is equal or greater than 0.6 T.

### Claim 2 (depends on 1)

The low-magnetic-field GaAs Quantum Hall Resistance sample as claimed in claim 1, wherein the thickness of the undoped AlxGa1-xAs isolation layer is in a range of 15 nm to 20 nm, the central magnetic field of the Quantum Hall Resistance plateau 2 is 7.6 T, and a magnetic field range corresponding to the Quantum Hall Resistance plateau 2 starts from 7.3 T and ends at 7.9 T.

### Claim 3 (depends on 1)

The low-magnetic-field GaAs Quantum Hall Resistance sample as claimed in claim 1, wherein a resistance value reproduced at the central magnetic field of the Quantum Hall Resistance plateau 2 is 12906.4037 ohms (Ω), and a relative measurement uncertainty is less than 2×10−8.

### Claim 4 (depends on 1)

The low-magnetic-field GaAs Quantum Hall Resistance sample as claimed in claim 1, wherein an impurity concentration of the high-purity GaAs layer is on an order of 1013 per cubic centimeter (1013/cm3), and a thickness of the high-purity GaAs layer is in a range of 380 nm to 420 nm; the two-dimensional electron gas layer is formed at a contact surface between the high-purity GaAs layer and the undoped AlxGa1-xAs isolation layer, a thickness of the two-dimensional electron gas layer is in a range of 9 nm to 11 nm, the carrier concentration of the two-dimensional electron gas layer is in a range of 3.0×1017/cm2 to 3.8×1017/cm2, and a carrier mobility of the two-dimensional electron gas layer is in a range of 1.0×105 cm2/(V·s) to 4.0×105 cm2/(V·s).

### Claim 5 (depends on 1)

The low-magnetic-field GaAs Quantum Hall Resistance sample as claimed in claim 1, wherein the GaAs/AlGaAs superlattice layer is configured to isolate impurities in the GaAs isolation layer, the GaAs/AlGaAs superlattice layer comprises a structure formed by alternately growing a GaAs material and a AlGaAs material for 20 cycles, and a thickness of the GaAs isolation layer is in a range of 200 nm to 500 nm.

### Claim 6 (depends on 1)

The low-magnetic-field GaAs Quantum Hall Resistance sample as claimed in claim 1, wherein a thickness of the Si-doped AlxGa1-xAs layer is in a range of 45 nm to 55 nm, a doping concentration of Si in the Si-doped AlxGa1-xAs layer is in a range of 8×1017/cm3 to 9×1017/cm3, and a thickness of the GaAs surface layer is in a range of 9 nm to 11 nm.

### Claim 7 (depends on 1)

The low-magnetic-field GaAs Quantum Hall Resistance sample as claimed in claim 1, wherein a periphery of the GaAs surface layer is provided with a plurality of metal electrodes connected to the GaAs surface layer, a material of each of the plurality of metal electrodes is an Au/Ge/Ni alloy, the Au/Ge/Ni alloy forms an ohmic contact with the two-dimensional electron gas layer, and a weight percentage (wt %) ratio of Au:Ge:Ni in the Au/Ge/Ni alloy is 88:8:4; and the plurality of metal electrodes comprises three pairs of voltage terminals arranged transversely and a pair of current terminals arranged longitudinally.

### Claim 8 (depends on 1)

A preparation method of the low-magnetic-field GaAs Quantum Hall Resistance sample as claimed in claim 1, comprising:
step 1, removing an oxide layer from the GaAs substrate;
step 2, growing the GaAs heterojunction material by a molecular beam epitaxy;
step 3, performing lithography on the GaAs heterojunction material to make the GaAs heterojunction material be in a Hall bar shape;
step 4, removing an oxide layer from the GaAs heterojunction material in the Hall bar shape;
step 5, depositing an Au/Ge/Ni electrode layer by an electron beam evaporation;
step 6, performing a rapid thermal annealing to form an ohmic contact; and
step 7, sealing.

### Claim 9 (depends on 8)

The preparation method as claimed in claim 8, wherein the step 1 specifically comprises:
placing the GaAs substrate in an environment of 580° C. to remove the oxide layer, and determining whether the oxide layer has been removed based on an infrared temperature of the GaAs substrate and changes in a reflection high-energy electron diffraction (RHEED) pattern.

### Claim 10 (depends on 8)

The preparation method as claimed in claim 8, wherein the step 2 specifically comprises: loading Ga, As, and Al materials required for growth of GaAs/AlGaAs into a source furnace, and sequentially growing the GaAs isolation layer, the GaAs/AlGaAs superlattice layer, the high-purity GaAs layer, the undoped AlxGa1-xAs isolation layer, the Si-doped AlxGa1-xAs layer, and the GaAs surface layer by controlling turning-on and turning-off and time of a front baffle of the source furnace; wherein the two-dimensional electron gas layer with a thickness of 10 nm is formed at an contact surface between the high-purity GaAs layer and the undoped AlxGa1-xAs isolation layer;
wherein the step 3 specifically comprises: performing spin coating, soft baking, exposure, development, etching, and stripping on the GaAs heterojunction material to make the GaAs heterojunction material be in the Hall bar shape;
wherein the step 4 specifically comprises: soaking the GaAs heterojunction material in the Hall bar shape in a (NH4)2S saturated solution for 30 seconds, and then rinsing with deionized water and drying;
wherein the step 6 specifically comprises: using a rapid thermal annealing system, maintaining at a temperature environment of 445-455° C. with a protective gas of N2/H2 for 4-6 minutes (min), and then rapidly cooling down to form an Au/Ge/Ni alloy, and diffusing down the Au/Ge/Ni alloy to the two-dimensional electron gas layer to form the ohmic contact; and
wherein the step 7 specifically comprises: using a wire bonding machine to connect metal electrodes to pins through an aluminum wire.