# US 2026/0097428 A1 · Cold rolled steel sheet for hot-press forming having excellent surface quality, hot-press-formed member, and method for manufacturing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0097428 A1
- Document ID: US20260097428A1
- Status: Published application
- Kind: A1
- Application number: 19/105,470
- Filed: 2023-08-17
- Published: 2026-04-09
- Earliest claimed: 2022-08-22
- Assignees: Posco
- Applicants: Posco Co., Ltd
- Inventors: Sea-Woong Lee; Jin-Keun Oh; Seong-Woo Kim; Sang-Heon Kim; Sang-Cheol Lee; Kwon-Il Kim
- Web page: https://patentgrep.com/patent/US20260097428A1

## CPC

- B21D 22/022: {by heating the blank or stamping associated with heat treatment (C21D takes precedence)}
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 8/0278: involving a particular surface treatment (C21D8/0294 takes precedence)
- C21D 8/0426: {Hot rolling}
- C21D 8/0436: {Cold rolling}
- C21D 8/0463: {following hot rolling}
- C21D 9/46: for sheet metals
- C21D 9/48: deep-drawing sheets
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/20: with copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/44: with molybdenum or tungsten
- C22C 38/50: with titanium or zirconium
- C22C 38/54: with boron
- C22C 38/58: with more than 1.5% by weight of manganese
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C23C 28/04: only coatings of inorganic non-metallic material
- C21D 2211/002: Bainite
- C21D 2211/003: Cementite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- B21D: WORKING OR PROCESSING OF SHEET METAL OR METAL TUBES, RODS OR PROFILES WITHOUT ESSENTIALLY REMOVING MATERIAL; PUNCHING METAL (working or processing of wire B21F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

The present invention relates to a cold rolled steel sheet for hot-press forming, a hot-press-formed member, and a method for manufacturing same and, more specifically, to a cold rolled steel sheet for hot-press forming, having excellent surface quality, a hot-press-formed member, and a method for manufacturing same.

## Claims

### Claim at position 1

1-20. (canceled)

### Claim 21

A cold-rolled steel sheet comprising: a base steel sheet and a first oxide layer formed on the base steel sheet,
wherein the first oxide layer comprises two or more of Fe, Mn, Cr, and Si, and has a thickness of 5 to 500 nm.

### Claim 22 (depends on 21)

The cold-rolled steel sheet of claim 21, wherein the base steel sheet comprises, by wt %, 0.05 to 0.4% of C, 0.5 to 3.0% of Si, 0.3 to 5.0% of Cr, 0.01 to 4.0% of Mn, 0.001 to 0.4% of Al, 0.001 to 0.05% of P, 0.0001 to 0.02% of S, 0.001 to 0.02% of N, and a balance of Fe and other unavoidable impurities.

### Claim 23 (depends on 22)

The cold-rolled steel sheet of claim 22, wherein the base steel sheet comprises one or more of 0.001 to 0.4% of Ti, 0.001 to 0.4% of Nb, 0.001 to 0.4% of Zr, 0.001 to 0.4% of V, 0.0001 to 0.01% of B, 0.001 to 1.0% of Mo, 0.001 to 1.0% of W, 0.005 to 2.0% of Cu, 0.005 to 2.0% of Ni, 0.001 to 1.0% of Sb, 0.001 to 1.0% of Sn, and 0.0001 to 0.02% of REM.

### Claim 24 (depends on 21)

The cold-rolled steel sheet of claim 21, wherein a sum of contents of Si, Mn, and Cr in the first oxide layer is 30% or more in terms of wt %.

### Claim 25 (depends on 21)

The cold-rolled steel sheet of claim 21, wherein the cold-rolled steel sheet has a microstructure comprising 5 area % or more of ferrite and cementite.

### Claim 26

A member comprising: a base steel sheet; a first oxide layer formed on the base steel sheet; and a second oxide layer formed on the first oxide layer, wherein the first oxide layer comprises two or more of Fe, Mn, Cr, and Si, and the second oxide layer is formed of an Fe-based oxide and has a thickness of 0.1 to 10 μm.

### Claim 27 (depends on 26)

The member of claim 26, wherein the base steel sheet comprises, by wt %, 0.05 to 0.4% of C, 0.5 to 3.0% of Si, 0.3% or more and less than 5.0% of Cr, 0.01 to 4.0% of Mn, 0.001 to 0.4% of Al, 0.001 to 0.05% of P, 0.0001 to 0.02% of S, 0.001 to 0.02% of N, and a balance of Fe and other unavoidable impurities.

### Claim 28 (depends on 27)

The member of claim 27, wherein the base steel sheet comprises one or more of 0.001 to 0.4% of Ti, 0.001 to 0.4% of Nb, 0.001 to 0.4% of Zr, 0.001 to 0.4% of V, 0.0001 to 0.01% of B, 0.001 to 1.0% of Mo, 0.001 to 1.0% of W, 0.005 to 2.0% of Cu, 0.005 to 2.0% of Ni, 0.001 to 1.0% of Sb, 0.001 to 1.0% of Sn, and 0.0001 to 0.02% of REM.

### Claim 29 (depends on 26)

The member of claim 26, wherein a sum of contents of Si, Mn, and Cr in the second oxide layer is less than 30% in terms of wt %.

### Claim 30 (depends on 26)

The member of claim 26, wherein the member has a microstructure comprising martensite or bainite as a main phase.

### Claim 31 (depends on 26)

The member of claim 26, wherein a tensile strength of the member is 500 MPa or more.

### Claim 32

A manufacturing method of a cold-rolled steel sheet, comprising:
reheating a steel slab;
hot rolling the reheated steel slab;
cooling and coiling the hot-rolled steel sheet;
cold rolling the coiled steel sheet; and
performing continuous annealing on the cold-rolled steel sheet,
wherein during the continuous annealing, a temperature increase rate at an atmosphere temperature of room temperature to 700° C. is 3.0 to 20.0° C./s, a temperature increase rate at an atmosphere temperature of 700 to 800° C. is 0.08 to 1.5° C./s, a temperature increase rate at an atmosphere temperature of 800 to 900° C. is 0.01 to 1.5° C./s, and a temperature increase rate at an atmosphere temperature of 900 to 1,000° C. is 0.01 to 1.0° C./s.

### Claim 33 (depends on 32)

The manufacturing method of claim 32, wherein the steel slab comprises, by wt %, 0.05 to 0.4% of C, 0.5 to 3.0% of Si, 0.3 to 5.0% of Cr, 0.01 to 4.0% of Mn, 0.001 to 0.4% of Al, 0.001 to 0.05% of P, 0.0001 to 0.02% of S, 0.001 to 0.02% of N, and a balance of Fe and other unavoidable impurities.

### Claim 34 (depends on 33)

The manufacturing method of claim 33, wherein the steel slab comprises one or more of 0.001 to 0.4% of Ti, 0.001 to 0.4% of Nb, 0.001 to 0.4% of Zr, 0.001 to 0.4% of V, 0.0001 to 0.01% of B, 0.001 to 1.0% of Mo, 0.001 to 1.0% of W, 0.005 to 2.0% of Cu, 0.005 to 2.0% of Ni, 0.001 to 1.0% of Sb, 0.001 to 1.0% of Sn, and 0.0001 to 0.02% of REM.

### Claim 35 (depends on 32)

The manufacturing method of claim 32, wherein the reheating is performed in a temperature range of 1,000 to 1,300° C.,
the hot rolling is performed at a finish rolling temperature of Ar3 to 1,000° C.,
the coiling is performed in a temperature range of Ms to 750° C., and
the cold rolling is performed at a reduction ratio of 30 to 80%.

### Claim 36 (depends on 32)

The manufacturing method of claim 32, wherein the continuous annealing is performed in a steel sheet temperature range of 700 to 900° C., and a continuous annealing time is 1 to 1,000 seconds.

### Claim 37 (depends on 32)

A manufacturing method of a member, comprising:
performing a heat treatment on the cold-rolled steel sheet of claim 32; and
performing hot press forming on the heat-treated steel sheet and then cooling the hot press formed steel sheet,
wherein during the heat treatment, an A value defined in the following Relational Expression 1 is 0.6 to 1.0:
A
=
(
T
+
0.2
t
)
/
1
,
TagBox[",", "NumberComma", Rule[SyntaxForm, "0"]]
210
[
Relational
⁢
Expression
⁢
1
]
where T represents a heating temperature and a unit thereof is ° C., and t represents a total heating time and a unit thereof is a second.

### Claim 38 (depends on 37)

The manufacturing method of claim 37, wherein during the heat treatment, the heating is performed to the heating temperature at an atmosphere temperature increase rate of 1 to 1,000° C./s.

### Claim 39 (depends on 37)

The manufacturing method of claim 37, wherein during the heat treatment, the heating temperature is 700 to 1,000° C., and the heating time is 150 to 1,000 seconds.

### Claim 40 (depends on 37)

The manufacturing method of claim 37, wherein after the hot press forming, during the cooling, the cooling is performed to an Mf temperature or lower at a cooling rate of 10 to 1,000° C./s.