# US 2026/0088285 A1 · Anode active material for lithium secondary battery and lithium secondary battery including the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0088285 A1
- Document ID: US20260088285A1
- Status: Published application
- Kind: A1
- Application number: 19/408,362
- Filed: 2025-12-04
- Published: 2026-03-26
- Earliest claimed: 2022-06-21
- Assignees: SK On Co., Ltd.; SK Innovation Co., Ltd.
- Applicants: SK On Co., Ltd.; SK Innovation Co., Ltd.
- Inventors: Young Mo YANG; Joon Hyung MOON; Do Ae YU; Ju Ho CHUNG; Jae Young CHOI
- Web page: https://patentgrep.com/patent/US20260088285A1

## CPC

- H01M 4/0428: {Chemical vapour deposition}
- H01M 4/366: {as layered products}
- H01M 4/133: Electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 4/134: Electrodes based on metals, Si or alloys
- H01M 4/1393: of electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 4/1395: of electrodes based on metals, Si or alloys
- H01M 4/386: {Silicon or alloys based on silicon}
- H01M 4/485: of mixed oxides or hydroxides for inserting or intercalating light metals, e.g. LiTi2O4 or LiTi2OxFy (H01M4/505, H01M4/525 take precedence)
- H01M 4/583: Carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 2004/027: {Negative electrodes}
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

An anode active material for a secondary battery includes a plurality of composite particles. The composite particles include carbon-based particles containing pores therein. A silicon-containing coating layer is formed inside the pores or on a surface of the carbon-based particles. A surface oxide layer is formed on the silicon-containing coating layer. The surface oxide layer contains silicon oxide. A silicon oxidation number ratio of the composite particle is predefined.

## Claims

### Claim 1

A method of preparing an anode active material for a lithium secondary battery, comprising:
heating a carbon-based particle including pores together with a silicon source to form a silicon-containing coating layer inside the pores or on a surface of the carbon-based particle; and
heat-treating the carbon-based particle on which the silicon-containing coating layer is formed while supplying an oxygen gas to form a composite particle including a surface oxide layer formed on the silicon-containing coating layer, the surface oxide layer containing silicon oxide,
wherein a silicon oxidation number ratio defined by Equation 1 of the composite particles is 0.6 or less:
silicon
⁢
oxidation
⁢
number
⁢
ratio
=
O
B
/
Os
[
Equation
⁢
1
]
where, in Equation 1, OS is an oxidation number of silicon included in the silicon-containing coating layer measured by an X-ray photoelectron spectroscopy (XPS), and OS is an oxidation number of silicon included in the surface oxide layer measured by the XPS.

### Claim 2 (depends on 1)

The method of claim 1, wherein the heat-treating is performed at a temperature from 100° C. to 250° C. to form the surface oxide layer.

### Claim 3 (depends on 1)

The method of claim 1, wherein the silicon source comprises silane injected into a CVD coater at a flow rate of 50 mL/min to 100 mL/min.

### Claim 4 (depends on 1)

The method of claim 1, wherein forming the silicon-containing coating layer comprises raising a temperature at a heating rate of 5° C./min to 20° C./min.

### Claim 5 (depends on 1)

The method of claim 1, wherein the silicon-containing coating layer is formed by maintaining the temperature at 200° C. for about 2 hours during the chemical vapor deposition.

### Claim 6 (depends on 1)

The method of claim 1, wherein a high-concentration oxygen gas is injected into a CVD coater at a flow rate of 50 mL/min to 100 mL/min during formation of the surface oxide layer.

### Claim 7 (depends on 1)

The method of claim 1, wherein the forming of the surface oxide layer comprises raising a temperature at a heating rate of 5° C./min to 20° C./min.

### Claim 8 (depends on 1)

The method of claim 1, wherein oxidizing the deposited silicon surface comprises maintaining the temperature at 100° C. for about 1 hour.

### Claim 9 (depends on 1)

The method of claim 1, wherein OS is obtained by substituting a first value, obtained by subtracting 99.6 eV from a binding energy of silicon included in the silicon-containing coating layer measured by the XPS, into a silicon oxidation number calibration curve, and
OS is obtained by substituting a second value, obtained by subtracting 99.6 eV from a binding energy of silicon included in the surface oxide layer measured by the XPS, into the silicon oxidation number calibration curve.

### Claim 10 (depends on 9)

The method of claim 9, wherein the silicon oxidation number calibration curve is obtained by connecting points corresponding to Si0, Si1+, Si2+, Si3+ and Si4+ with a shortest distance between neighboring points in a graph in which an x-axis represents oxidation numbers of silicon and a y-axis represents the first and second values obtained by subtracting 99.6 eV from the binding energies of silicon measured by the XPS.

### Claim 11 (depends on 1)

The method of claim 1, wherein a distance between a surface of the composite particle and the silicon-containing coating layer is 100 nm to 700 nm, and a distance between the surface of the composite particle and the surface oxide layer formed on the silicon-containing coating layer is 10 nm or less.

### Claim 12 (depends on 1)

The method of claim 1, wherein OB is in a range from 1.2 to 2.0, and OS is in a range from 3.0 to 3.6.

### Claim 13 (depends on 1)

The method of claim 1, wherein an oxygen content ratio defined by Equation 2 is 0.4 or less:
oxygen
⁢
content
⁢
ratio
=
C
B
/
C
S
[
Equation
⁢
2
]
where, in Equation 2, CB is a percentage (at %) of the number of oxygen atoms included in the silicon-containing coating layer relative to a sum of the number of atoms included both in the silicon-containing coating layer and in the surface oxide layer measured by the XPS, CS is a percentage (at %) of the number of oxygen atoms included in the surface oxide layer relative to the sum of the number of atoms included both in the silicon-containing coating layer and in the surface oxide layer measured by the XPS.

### Claim 14 (depends on 13)

The method of claim 13, wherein CB is in a range from 8 at % to 15 at %, and CS is in a range from 15 at % to 34 at %.