# US 2026/0085737 A1 · Friction material composition and fabricating articles therefrom

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0085737 A1
- Document ID: US20260085737A1
- Status: Published application
- Kind: A1
- Application number: 19/109,721
- Filed: 2023-08-09
- Published: 2026-03-26
- Earliest claimed: 2022-09-08
- Applicants: Gharda Chemicals Limited
- Inventors: Prakash D. TRIVEDI; Jayashree BIJWE; Bhaskaranand BHATT; Umesh MARATHE
- Web page: https://patentgrep.com/patent/US20260085737A1

## CPC

- F16D 69/026: {containing fibres}
- F16D 69/023: {Composite materials containing carbon and carbon fibres or fibres made of carbonizable material}
- F16D 2200/0086: Moulding materials together by application of heat and pressure
- F16D 2200/0095: Mixing an aqueous slurry of fibres with a binder, e.g. papermaking process
- F16D: COUPLINGS FOR TRANSMITTING ROTATION; CLUTCHES; BRAKES

## Abstract

The present disclosure relates to a friction material composition comprising reactive poly aryl ether ketone (R-PAEK) as a binder. The present disclosure further relates to a process for the preparation of a friction material composition. Furthermore, the present disclosure relates to a process for the fabrication of an article by using the friction material composition. The friction material composition of the present disclosure does not require post curing while manufacturing brake pads. Further, the article fabricated by using the friction material composition of the present disclosure has longer shelf life and do not evolve noxious by-products and possesses superior physical and tribological properties.

## Claims

### Claim 1

A friction material composition comprising:
(i) a first mixture that includes;
2 mass % to 25 mass % of at least one fibrous material;
2 mass % to 25 mass % of at least one friction modifier; and
8 mass % to 45 mass % of at least one functional filler; and
(ii) a second mixture that includes;
13 mass % to 25 mass % of at least one inert filler; and
3 mass % to 15 mass % of at least one binder,
wherein a mass ratio of said first mixture to said second mixture is in the range of 1:0.1 to 1:0.5,
wherein said mass % of each component is with respect to the total mass of said friction material.

### Claim 2 (depends on 1)

The friction material composition as claimed in claim 1, wherein said fibrous material is at least one selected from the group consisting of rockwool fibers, polyacrylonitrile (PAN) fibers, aramid fibers, glass fibers, carbon fibers, polyester fibers, polyimide fibers and wollastonite fibers.

### Claim 3 (depends on 1)

The friction material composition as claimed in claim 1, wherein said friction modifier is at least one selected from the group consisting of zircon, natural graphite, silicon carbide, zirconium silicate, alumina, silica, mullite, tin sulphide and petroleum coke.

### Claim 4 (depends on 1)

The friction material composition as claimed in claim 1, wherein said functional filler is at least one selected from the group consisting of synthetic hydrated calcium silicate (Promaxon-D), potassium titanate, stainless steel particles 410, vermiculite, mica, attapulgite, talc, molybdenum trioxide, kaolin, flyash and hexagonal boron nitride.

### Claim 5 (depends on 1)

The friction material composition as claimed in claim 1, wherein said inert filler is at least one selected from the group consisting of barite and calcium carbonate.

### Claim 6 (depends on 1)

The friction material composition as claimed in claim 1, wherein said binder is at least one selected from the group consisting of reactive poly aryl ether ketone (R-PAEK), polybenzoxazine resin, thermosetting polymer such as phenolic resin and epoxy resin.

### Claim 7 (depends on 6)

The friction material composition as claimed in claim 6, wherein said reactive poly aryl ether ketone (R-PAEK) has a particle size (D50) in the range of 5 microns to 60 microns.

### Claim 8

A process for the preparation of a friction material composition, said process comprising the following steps:
(i) mixing at least one fibrous material with at least one inert filler at a first predetermined stirring speed for a first predetermined time period to obtain a first mixture;
(ii) separately, mixing at least one friction modifier, at least one functional filler and at least one binder at a second predetermined stirring speed for a second predetermined time period to obtain a second mixture; and
(iii) mixing said first mixture and said second mixture at a third predetermined stirring speed for a third predetermined time period to obtain said friction material composition.

### Claim 9 (depends on 8)

The process as claimed in claim 8, wherein said fibrous material is at least one selected from the group consisting of rockwool fibers, polyacrylonitrile (PAN) fibers, aramid fibers, glass fibers, carbon fibers, polyester fibers, polyimide fibers and wollastonite fibers.

### Claim 10 (depends on 8)

The process as claimed in claim 8, wherein said inert filler is at least one selected from the group consisting of barite and calcium carbonate.

### Claim 11 (depends on 8)

The process as claimed in claim 8, wherein said first and said second predetermined stirring speed is independently in the range of 200 rpm to 400 rpm.

### Claim 12 (depends on 8)

The process as claimed in claim 8, wherein said first predetermined time period is in the range of 2 minutes to 25 minutes.

### Claim 13 (depends on 8)

The process as claimed in claim 8, wherein said friction modifier is at least one selected from the group consisting of zircon, natural graphite, silicon carbide, zirconium silicate, alumina, silica, mullite, tin sulphide and petroleum coke.

### Claim 14 (depends on 8)

The process as claimed in claim 8, wherein said functional filler is at least one selected from the group consisting of synthetic hydrated calcium silicate (Promaxon-D), potassium titanate, stainless steel particles 410, vermiculite, mica, attapulgite, talc, molybdenum trioxide, kaolin, flyash and hexagonal boron nitride.

### Claim 15 (depends on 8)

The process as claimed in claim 8, wherein said binder is at least one selected from the group consisting of reactive poly aryl ether ketone (R-PAEK), polybenzoxazine resin, thermosetting polymer such as phenolic resin and epoxy resin.

### Claim 16 (depends on 15)

The process as claimed in claim 15, wherein said reactive poly aryl ether ketone (R-PAEK) has a particle size (D50) in the range of 5 microns to 60 microns.

### Claim 17 (depends on 8)

The process as claimed in claim 8, wherein said second predetermined time period and said third predetermined time period is independently in the range of 2 minutes to 10 minutes.

### Claim 18 (depends on 8)

The process as claimed in claim 8, wherein said third predetermined stirring speed is in the range of 2500 rpm to 3000 rpm.

### Claim 19 (depends on 1)

A process for the fabrication of an article by using said friction material composition as claimed in claim 1, said process comprising the following steps:
a. drying said friction material composition at a temperature in the range of 60° C. to 90° C. to obtain a dried friction material composition;
b. preforming said dried friction material composition at a pressure in the range of 1 MPa to 3 MPa to obtain at least one preform;
c. placing said preform into a mold cavity followed by heating to a temperature in the range of 400° C. to 450° C. for a time period in the range of 2 minutes to 10 minutes to obtain a heated preform,
wherein said mold cavity is fixed into a compression molding machine and preloaded with adhesive-applied backplates,
d. applying a pressure in the range of 80 bars to 120 bars with 5 cycles of intermittent breathings to said heated preform for a time period in the range of 5 hours to 10 hours to obtain a fabricated article; and
e. cooling said fabricated article to a temperature in the range of 20° C. to 30° C. followed by removing said fabricated article from said mold cavity.